PERMABOND 268

Harmonization Code : 3506.10.00.00 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg

PERMABOND 268

Main features

  • 0.43 mm Maximum Gap Fill
  • 5 to 10-Second Handling Time
  • MIL-A-46050C Type II Class 3 Approval

Product Description

PERMABOND® 268 is a single-part, medium-high-viscosity ethyl cyanoacrylate adhesive developed for rapid bonding where greater gap-filling capability is required than with conventional low-viscosity instant adhesives. It bonds metals, ceramics, plastics and elastomers, including polyacetal and passivated metal surfaces. The adhesive requires no mixing, fixtures in approximately 5–10 seconds on selected tested substrates and reaches full strength after 24 hours. Its documented maximum gap fill is 0.43 mm.

Key features

  • Medium-high viscosity: A typical viscosity of 1,200–2,400 mPa·s at 25°C supports controlled application and greater gap fill than lower-viscosity cyanoacrylates.
  • Rapid fixture: Reaches the documented 0.3 N/mm² handling-strength threshold in approximately 5–10 seconds on steel, Buna-N rubber and phenolic.
  • 0.43 mm maximum gap fill: Supports close-fitting assemblies with larger clearances than conventional instant adhesives.
  • Broad substrate capability: Documented for metals, ceramics, plastics and elastomers, including polyacetal and passivated metals.
  • Military specification approval: Approved to MIL-A-46050C Type II Class 3 for existing designs.

Suitable for

  • Rapid assembly of metal, ceramic, plastic and elastomer components
  • Joints requiring controlled application across gaps up to 0.43 mm
  • Bonding polyacetal and passivated metal surfaces

Application videos

Product Family

PERMABOND 268

Loading pricing…

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Appearance
Appearance at room temperature.
Liquid
Color
The color
Colourless
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.1
Physical Properties
Viscosity
Viscosity is a measurement of a fluid’s resistance to flow. Viscosity is commonly measured in centiPoise (cP). One cP is defined as the viscosity of water and all other viscosities are derived from this base. MPa is another common unit with a 1:1 conversion to cP. A product like honey would have a much higher viscosity -around 10,000 cPs- compared to water. As a result, honey would flow much slower out of a tipped glass than water would. The viscosity of a material can be decreased with an increase in temperature in order to better suit an application
1,200-2,400 mPa.s
Thermal Properties
Thermal Conductivity
Thermal conductivity describes the ability of a material to conduct heat. It is required by power packages in order to dissipate heat and maintain stable electrical performance. Thermal conductivity units are [W/(m K)] in the SI system and [Btu/(hr ft °F)] in the Imperial system.
0.1 W/m.K

Additional Information

Gap-filling cyanoacrylate adhesive

PERMABOND® 268

PERMABOND® 268 is a single-part, medium-high-viscosity ethyl cyanoacrylate adhesive for rapid assembly where increased gap-filling capability is needed. It bonds metals, ceramics, plastics and elastomers and is specifically documented for polyacetal and passivated metal surfaces.

Single-part Ethyl cyanoacrylate Medium-high viscosity 0.43 mm gap fill Fast fixture
PERMABOND 268 medium-high-viscosity cyanoacrylate adhesive bottle and packaging

Medium-high-viscosity instant adhesive for rapid bonding and increased gap fill.

As supplied

Uncured adhesive properties

The medium-high-viscosity formulation supports controlled placement and greater gap fill than conventional low-viscosity cyanoacrylates. Viscosity describes the uncured adhesive at 25°C and does not independently establish wetting or bond strength.

Chemical composition
Ethyl cyanoacrylate
Single-part reactive adhesive.
Appearance
Colorless
Uncured liquid appearance.
Viscosity
1,200–2,400 mPa·s
Typical at 25°C.
Specific gravity
1.1
Typical uncured-material value.
Typical uncured adhesive data
Property Typical value Condition
Component  One No mixing required
Chemical composition Ethyl cyanoacrylate -
Appearance Colorless liquid -
Viscosity 1,200–2,400 mPa·s 25°C
Specific gravity 1.1 -

Values are typical guideline data and are not guaranteed product specifications.

Cure behavior

Gap fill, fixture time and full strength

Fixture or handling time is defined as the time needed to reach 0.3 N/mm² shear strength. It must remain separate from the 24-hour period stated for full strength.

Maximum gap fill
0.43 mm
Documented maximum, equivalent to 0.017 in.
Fixture threshold
0.3 N/mm²
Shear-strength definition used for handling time.
Fixture time
5–10 sec
On steel, Buna-N rubber and phenolic test substrates.
Full strength
24 h
Typical room-temperature strength-development period.
Substrate-specific handling time
Substrate Typical fixture time Definition
Steel 5–10 seconds Time to 0.3 N/mm² shear strength
Buna-N rubber 5–10 seconds Time to 0.3 N/mm² shear strength
Phenolic 5–10 seconds Time to 0.3 N/mm² shear strength

Temperature, humidity, substrate chemistry and joint gap affect fixture time. Larger gaps and acidic surfaces may slow cure development.

Processing

Surface preparation and bonding process

PERMABOND 268 cures rapidly after assembly. Prepare and align the components before dispensing, apply the adhesive sparingly and avoid moving the joint while handling strength develops.

Clean and dry: Remove grease, dust and contamination. Acetone or isopropanol may be used where compatible with the substrate and process.
Prepare oxide-forming metals: Aluminum, copper and copper alloys may benefit from light abrasion to remove surface oxide before final cleaning.
Apply sparingly: Dispense the adhesive onto one surface. Use enough material to fill the intended joint without unnecessary squeeze-out.
Assemble immediately: Bring the components together quickly in the correct alignment and apply enough pressure to distribute the adhesive through the joint.
Hold without movement: Do not disturb or reposition the components until adequate handling strength has developed.
Process diagram showing cleaning, optional abrasion, PERMABOND 268 dispensing, component assembly, joint pressure and rapid fixture

Recommended visual: substrate cleaning, optional metal abrasion, controlled dispensing, immediate alignment, joint pressure and fixture.

Large gaps or acidic surfaces

Larger gaps and acidic surfaces may reduce cure speed. Permabond C Surface Activator or Permabond QFS 16 may be evaluated where faster cure is needed.

Difficult or porous surfaces

A compatible Permabond activator may be considered for porous or difficult-to-bond surfaces, subject to application testing.

Low-surface-energy polymers

Polypropylene, polyethylene, PTFE and silicone require Permabond Polyolefin Primer before adhesive application.

Storage and handling

Store PERMABOND 268 at 2–7°C. Allow the closed bottle to reach room temperature before opening to reduce the risk of condensation entering the container and shortening shelf life. Use appropriate industrial hygiene practices and consult the current regional safety documentation before handling.

Bonded-joint performance

Substrate-specific shear strength

The following ISO 4587 values apply to the specified test substrates and conditions. Actual performance depends on substrate grade, preparation, joint gap, cure and test configuration.

Typical cured shear-strength results
Substrate Typical shear strength Test context
Steel 20–22 N/mm² (2,900–3,200 psi) ISO 4587
ABS Greater than 6 N/mm² (>870 psi) Substrate failure reported
PVC Greater than 6 N/mm² (>870 psi) Substrate failure reported
Polycarbonate Greater than 5 N/mm² (>725 psi) Substrate failure reported

A substrate-failure result means the tested substrate failed before the adhesive joint under that particular test configuration. It is not a universal minimum bond-strength rating.

Cured adhesive

Mechanical and thermal properties

These values describe the cured adhesive or a specified laboratory test configuration. They do not independently establish complete bonded-assembly performance.

Impact strength
3–5 kJ/m²
ASTM D950.
Thermal conductivity
0.1 W/(m·K)
Typical cured-material value.
Thermal expansion
90 × 10−6 mm/mm/°C
Typical cured-material coefficient.
Hardness
85 Shore D
ISO 868.
Typical cured adhesive data
Property Typical value Test Method
Impact strength 3–5 kJ/m² (1.4-2.4 ft-lb/in²) ASTM D950
Coefficient of thermal expansion 90 × 10−6 mm/mm/°C -
Thermal conductivity 0.1 W/(m·K) -
Hardness 85 Shore D ISO 868

Temperature and environmental guidance

The cured adhesive may be exposed to approximately −55°C, depending on the bonded materials. It may tolerate higher temperatures briefly during operations such as paint baking or wave soldering when the joint is not heavily stressed.

PERMABOND 268 is not recommended for contact with strong oxidizing materials or polar solvents. Temperature and chemical resistance should be confirmed in the intended substrate system, joint geometry, exposure duration and load condition.

Applications

Rapid assembly with increased gap fill

PERMABOND 268 is relevant where fast fixture, controlled adhesive placement and accommodation of larger close-fitting joint gaps are important process considerations.

Metal components

Metal and passivated-metal assembly

The adhesive is documented for metal bonding and can be used on passivated metal surfaces. Its medium-high viscosity supports controlled application where joint clearances are greater than those suited to very low-viscosity cyanoacrylates.

Polyacetal and engineering plastic components

Polyacetal and engineering plastics

PERMABOND 268 is specifically identified for difficult-to-bond plastics such as polyacetal. Published test results also support evaluation on ABS, PVC and polycarbonate, subject to grade and surface-condition testing.

Elastomer and ceramic components

Elastomer and ceramic components

The product is documented for elastomers and ceramics. Fixture time and final bond performance remain dependent on formulation, surface condition, joint gap and actual assembly geometry.

Application videos

Cyanoacrylate application and surface preparation

These videos provide complementary guidance. The first demonstrates the general sequence for applying and assembling cyanoacrylate-bonded parts, while the second explains surface preparation considerations that can affect bond consistency.

Cyanoacrylate directions for use

Learn the general sequence for dispensing a cyanoacrylate adhesive, aligning the components, applying pressure and allowing the joint to fixture without movement.

Surface preparation directions

Review cleaning, contamination removal and surface-conditioning steps that can influence adhesive wetting, cure and bonded-joint consistency.

Next steps

Evaluate PERMABOND® 268 for your gap-filling rapid-assembly process

Contact Krayden to review joint clearance, substrate preparation, dispensing control, fixture-time requirements, activator or primer selection and application-specific testing for metal, plastic, ceramic or elastomer assemblies.

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers