Loctite EA 9395 AERO EPOXY ADHESIVE

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

Loctite EA 9395 AERO EPOXY ADHESIVE

Main features

  • 1,200 psi Lap Shear
  • Thixotropic Application Control
  • Ambient-Temperature Bonding Cure

Product Description

LOCTITE® EA 9395 AERO Epoxy Paste Adhesive is a two-component, ambient-temperature-curing epoxy adhesive with a thixotropic paste consistency and non-metallic filler. The mixed material is suitable for potting, filling and fairing applications and may be used with composite substrates, including applications where radar-absorbing material or structure considerations are important. After a five-day cure at 77°F/25°C, the adhesive provides a typical tensile lap shear strength of 4,300 psi (29.7 MPa) at 77°F/25°C and retains 1,200 psi (8.3 MPa) at 350°F/177°C on phosphoric-acid-anodized 2024-T3 AlClad aluminum under ASTM D1002 testing. The system uses a 100:17 mix ratio by weight and has a pot life of 95–100 minutes for a 450 g mass at 77°F/25°C.

Key features

  • High-temperature strength retention: Retains a typical tensile lap shear strength of 1,200 psi (8.3 MPa) at 350°F/177°C under the documented ASTM D1002 test configuration.
  • Thixotropic, non-metallic formulation: Supports paste application for potting, filling and fairing without the use of metallic filler.
  • Ambient-temperature cure: Develops normal performance after five days at 77°F/25°C, with an alternative cure of one hour at 150°F/66°C.

Applications / Suitable for

  • Potting applications
  • Filling and fairing
  • Composite-substrate assemblies
  • Applications involving RAM/RAS considerations

Technical Specifications

Physical Properties
Viscosity (Part A)
710,000 mPa.s
Viscosity (Part B)
36,000 mPa.s
General Properties
Mix Ratio
The amount of a constituent divided by the total amount of all other constituents in a mixture
100:17

Additional Information

Technical properties

As-supplied / before-processing properties

Typical uncured component and mixed-material properties. Component identity, temperature and Brookfield test conditions are retained where supplied.

Property Value Unit Method / condition
Product form Two-component thixotropic epoxy paste adhesive — As supplied
Filler type Non-metallic — Formulation characteristic
Color, Part A Light blue — Uncured
Color, Part B Olive brown-black — Uncured
Color, mixed Gray-blue — Immediately after mixing
Viscosity, Part A 7,100 poise 77°F; Brookfield HBT, spindle 7 at 20 rpm
Viscosity, Part A 710 Pa·s 25°C; Brookfield HBT, spindle 7 at 2.1 rad/s
Viscosity, Part B 360 poise 77°F; Brookfield HBT, spindle 4 at 20 rpm
Viscosity, Part B 36 Pa·s 25°C; Brookfield HBT, spindle 4 at 2.1 rad/s
Viscosity, mixed 1,000–3,000 poise 77°F; Brookfield HBT, spindle 5 at 20 rpm
Viscosity, mixed 100–300 Pa·s 25°C; Brookfield HBT, spindle 5 at 2.1 rad/s
Density, Part A 1.42 g/mL Uncured component
Density, Part B 1.00 g/mL Uncured component
Density, mixed 1.31 g/mL Mixed adhesive
Mix ratio, Part A:Part B 100:17 parts by weight Volume measurement is not recommended for structural applications unless precautions are taken to assure the correct ratio
Pot life 95–100 minutes 450 g mass at 77°F/25°C; ASTM D2471, water bath
Handling strength 24 hours At 77°F/25°C; full bond strength has not yet been attained
Standard cure schedule 5 days — 77°F/25°C; normal performance
Alternative cure schedule 1 hour — 150°F/66°C; normal performance
Shelf life, Part A 1 year Stored below 40°F/4°C or below 77°F/25°C
Shelf life, Part B 1 year Stored below 40°F/4°C or below 77°F/25°C
Technical properties

After-processing / final-state properties

Typical cured adhesive and bonded-joint properties. Cure schedules, substrates, surface preparation, test temperatures and methods are retained because these conditions materially affect the results.

Property Value Unit Method / condition
Tensile lap shear strength 2,300 / 15.8 psi / MPa Tested at −67°F/−55°C; ASTM D1002; cured 5 days at 77°F/25°C; 2024-T3 AlClad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear strength 4,300 / 29.7 psi / MPa Tested at 77°F/25°C; ASTM D1002; documented aluminum preparation and cure
Tensile lap shear strength 3,500 / 24.1 psi / MPa Tested at 180°F/82°C; ASTM D1002; documented aluminum preparation and cure
Tensile lap shear strength 3,000 / 20.7 psi / MPa Tested at 250°F/121°C; ASTM D1002; documented aluminum preparation and cure
Tensile lap shear strength 2,200 / 15.2 psi / MPa Tested at 300°F/149°C; ASTM D1002; documented aluminum preparation and cure
Tensile lap shear strength 1,200 / 8.3 psi / MPa Tested at 350°F/177°C; ASTM D1002; documented aluminum preparation and cure
T-peel strength 5–8 / 22–36 lb/in / N/25 mm 77°F/25°C; ASTM D1876; cured 5 days at 77°F/25°C; phosphoric-acid-anodized 2024-T3 AlClad aluminum
Bell peel strength 15 / 67 lb/in / N/25 mm 77°F/25°C; ASTM D3167; cured 5 days at 77°F/25°C; phosphoric-acid-anodized 2024-T3 AlClad aluminum
Service temperature Approximately 350 / 177 °F / °C Defined as the temperature at which the adhesive retains 1,000 psi/6.9 MPa by ASTM D1002
Tensile strength 8,070 / 55.6 psi / MPa 77°F/25°C; ASTM D638; 0.125 in/3.18 mm casting cured 5 days at 77°F/25°C
Tensile modulus 717 / 4,940 ksi / MPa 77°F/25°C; ASTM D638; documented casting and cure
Elongation at break 2.6 % 77°F/25°C; ASTM D638; documented casting and cure
Shore D hardness 90 Shore D 77°F/25°C
Glass transition temperature, Tg 163 / 73 °F / °C Tan delta by DMTA
Shear modulus, dry 224 / 1,543 ksi / MPa 77°F/25°C
Compressive strength 22,700 / 156.4 psi / MPa −67°F/−55°C; ASTM D695; cylindrical specimen 0.5 in/12.7 mm diameter × 1 in/25.4 mm
Compressive strength 14,000 / 96.5 psi / MPa 75°F/25°C; ASTM D695; documented cylindrical specimen
Compressive strength 10,100 / 69.6 psi / MPa 250°F/121°C; ASTM D695; documented cylindrical specimen
Compressive strength 6,800 / 46.9 psi / MPa 350°F/177°C; ASTM D695; documented cylindrical specimen
Compressive modulus 429 / 2,956 ksi / MPa 77°F/25°C; ASTM D695
Dielectric constant 4.22 — 0.1 kHz; ASTM D150
Dielectric constant 4.13 — 1.0 kHz; ASTM D150
Dielectric constant 3.97 — 10.0 kHz; ASTM D150
Dissipation factor 0.016 — 0.1 kHz; ASTM D150
Dissipation factor 0.021 — 1.0 kHz; ASTM D150
Dissipation factor 0.033 — 10.0 kHz; ASTM D150