LOCTITE EA 9359.3

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE EA 9359.3

Main features

  • 2:1 Controlled Mixing
  • 7-Day Cure Cycle
  • Humidity and Fluid Resistance

Product Description

LOCTITE EA 9359.3 AERO is a two-component structural epoxy paste adhesive with non-sag handling, integrated 0.13 mm glass beads for bondline thickness control, and a 2:1 dual-cartridge format with static mixer. The yellow Part A and blue Part B form a green mixed adhesive with a typical density of 1.12 g/mL. Pot life is mass-dependent at 25°C, ranging from 60 minutes for 100 g to 40 minutes for 450 g. The adhesive cures at room temperature or with an accelerated 1-hour cure at 82°C for small mixed quantities. Typical testing on phosphoric-acid-anodized 2024-T3 AlClad aluminum demonstrates tensile lap shear and T-peel performance, while the cured adhesive provides resistance to water, salt spray, and most organic fluids.

Key features

  • Controlled bondline thickness: Integrated 5 mil/0.13 mm glass beads help establish a defined adhesive layer.
  • Non-sag cartridge application: Supplied in a 2:1 dual cartridge with static mixer for controlled two-component dispensing.
  • Mass-dependent working window: Typical pot life at 25°C is 60 minutes for 100 g, 50 minutes for 200 g, and 40 minutes for 450 g.
  • Room-temperature or accelerated cure: Normal performance develops after 5–7 days at 25°C; a 1-hour cure at 82°C may be used for small mixed quantities.
  • Prepared-aluminum bond performance: Typical results at 25°C include 31.0 MPa tensile lap shear and 267 N/25 mm T-peel under the stated test conditions.

Suitable for

  • Structural bonding applications involving metals.
  • Bonding applications involving thermoplastics.
  • Bonding applications involving composite substrates.

Technical Specifications

General Properties
Color
The color
Yellow (Part A) / Blue (Part B)
Density (g)
1.16 (Part A) / 01.01 (Part B) g/cm3
Mix Ratio
The amount of a constituent divided by the total amount of all other constituents in a mixture
100:44 by weight
Physical Properties
Viscosity (Part A)
200,000 mPa.s
Viscosity (Part B)
100,000 mPa.s

Additional Information

Adhesives | Two-part structural epoxy paste

LOCTITE EA 9359.3 AERO

LOCTITE EA 9359.3 AERO is a two-component structural epoxy paste adhesive with integrated 0.13 mm glass beads for bondline control. The non-sag system is supplied in a 2:1 dual cartridge with static mixer and develops typical prepared-aluminum lap shear and T-peel performance after room-temperature cure. The cured adhesive also provides resistance to water, salt spray, and most organic fluids.

Two-part structural epoxy paste 0.13 mm glass-bead bondline control Non-sag paste 2:1 cartridge with static mixer 60-minute pot life for 100 g at 25°C Room-temperature or accelerated cure
LOCTITE EA 9359.3 AERO two-component epoxy adhesive cartridge

 

As supplied

As-Supplied Properties

Bondline control
0.13 mm
Integrated 5 mil glass beads provide a physical bondline-thickness control feature.
Cartridge format
2:1 dual cartridge
The product is offered with a static mixer for controlled two-component dispensing.

Values apply to the separate components or freshly mixed adhesive as identified. Viscosity values retain the stated instrument, spindle, speed, and temperature.

Property Value Unit / state Method / condition
Product form Two-component structural epoxy paste adhesive — Part A and Part B are mixed immediately before application
Color Yellow / blue / green Part A / Part B / mixed As supplied and after complete mixing
Part A viscosity 200 Pa·s 25°C; Brookfield HBT, spindle 7 at 2.1 rad/s
Part B viscosity 100 Pa·s 25°C; Brookfield HBT, spindle 6 at 2.1 rad/s
Density 1.16 / 1.01 / 1.12 g/mL Part A / Part B / mixed
Mix ratio by weight 100:44 Part A:Part B Maintain the stated component ratio
Mix ratio by volume 2:1 Part A:Part B Volume measurement is not recommended for structural applications unless ratio control is assured
Pot life - 100 g mass 60 minutes 25°C; ASTM D2471 in a water bath
Pot life - 200 g mass 50 minutes 25°C; ASTM D2471 in a water bath
Pot life - 450 g mass 40 minutes 25°C; ASTM D2471 in a water bath
Shelf life 1 year Part A and Part B at 25°C
Preparation, application, and cure

Processing and Cure

Control the component ratio, mixed mass, surface condition, assembly support, and cure schedule. The exotherm increases with mixed quantity, so batch size is a safety-critical processing parameter.

Surface preparation: Bonding surfaces should be clean, dry, and properly prepared before adhesive application.
Component mixing: Bring the separate components close to room temperature, combine Part A and Part B at the correct ratio, and mix thoroughly. Complete mixing is required.
Working time: At 25°C, typical pot life is 60 minutes for 100 g, 50 minutes for 200 g, and 40 minutes for 450 g. Working time decreases as mixed mass increases.
Assembly and handling: Apply the mixed adhesive, assemble the parts, and maintain contact until the adhesive is set. Handling strength develops after 24 hours at temperatures above 25°C; keep loads small because full bond strength has not yet developed.
Cure: Normal performance develops after 5–7 days at 25°C. For small mixed masses, accelerated cure up to 93°C may be used; 1 hour at 82°C provides complete cure.
Batch and cleanup control: Do not mix more than 450 g because uncontrolled exotherm and toxic fumes can occur. Remove excess uncured adhesive from equipment and work areas before it hardens, using an appropriate solvent under its safe-use instructions.
Storage and Handling

Keep the components tightly closed in their original containers in a cool, well-ventilated area away from heat, sparks, flame, and incompatible materials. Shelf life is 1 year at 25°C for Part A and Part B; store Part A at or below 25°C. Avoid mixing the components until the adhesive will be used immediately. For industrial use only; follow the current product-label and safety instructions for both components before handling.

Cured Material Properties

Tensile modulus
2,136 MPa
Typical at 25°C using ASTM D638 castings under the stated cure schedule.
Thermal conductivity
0.24 W/mK
Typical bulk-resin value tested using ASTM E1461.

These are typical bulk-material results. They are not guaranteed design values and should not be treated as assembled-joint performance without relevant joint testing.

Property Typical value Unit Method / condition
Tensile modulus 2,136 MPa 25°C; 3.18 mm castings; ASTM D638; cure 5 days at 25°C plus 1 hour at 93°C
Elongation at break 7.7 % 25°C; 3.18 mm castings; ASTM D638; cure 5 days at 25°C plus 1 hour at 93°C
Shear modulus - dry 1,027 MPa 25°C; RDS
Shear modulus - wet 613 MPa 25°C; RDS; wet exposure 30 days at 71°C and 95% RH
Glass transition temperature - 25°C cure, dry 51 °C Tan delta by DMTA
Glass transition temperature - 25°C cure, wet 66 °C Tan delta by DMTA; wet exposure 30 days at 71°C and 95% RH
Glass transition temperature - 93°C cure, dry 85 °C Tan delta by DMTA
Glass transition temperature - 93°C cure, wet 65 °C Tan delta by DMTA; wet exposure 30 days at 71°C and 95% RH
Specific heat 0.93 J/g ASTM E1461
Thermal conductivity 0.24 W/mK ASTM E1461
Compressive strength - 25°C cure 53.0 MPa Tested at 25°C on 12.7 × 25.4 mm cylinders; ASTM D695
Compressive strength - 93°C cure 145 MPa Tested at 25°C on 12.7 × 25.4 mm cylinders; ASTM D695

Performance Evidence

Typical mechanical results apply to the stated aluminum substrate, surface preparation, cure, test method, and temperature. Confirm performance for the intended substrate grade, bondline, joint geometry, production process, and service exposure.

Tensile lap shear across test temperature
Test temperature Typical result (psi) Typical result (MPa)
−55°C 4,000 27.6
25°C 4,500 31.0
82°C 2,000 13.8
93°C 1,000 6.9
ASTM D1002 after a 7-day cure at 25°C. Adherends: 2024-T3 AlClad aluminum, phosphoric-acid anodized per ASTM D3933.
T-peel strength
Typical result: 60 lb/in (267 N/25 mm) at 25°C.
ASTM D1876 after a 7-day cure at 25°C. Adherends: 2024-T3 AlClad aluminum, phosphoric-acid anodized per ASTM D3933.
Service-temperature definition and environmental resistance
Approximate service temperature is 93°C, defined as the temperature at which the adhesive retains 1,000 psi (6.9 MPa) tensile lap shear using ASTM D1002. The cured adhesive also provides resistance to water, salt spray, and most organic fluids. Exposure performance should be confirmed for the exact fluid, concentration, temperature, duration, substrate, and joint design.
The service-temperature value is a retained lap-shear criterion, not a guarantee of unchanged properties or long-term durability throughout all environments.
Supported bonding contexts

Applications

The adhesive may be evaluated for structural bonding across the substrate classes below. Confirm adhesion and durability on the exact material grade, finish, surface preparation, bondline, cure schedule, and operating environment.

Prepared metal components positioned for structural adhesive bonding
Metal bonding
Suitable for evaluation in structural metal-bonding applications. Typical lap-shear and T-peel values are specific to phosphoric-acid-anodized 2024-T3 AlClad aluminum and should not be generalized to other metals or finishes.
Thermoplastic components prepared for adhesive bonding
Thermoplastic bonding
Suitable for evaluation with thermoplastic substrates where a two-part, non-sag structural adhesive and controlled bondline are relevant. Verify wetting, adhesion, cure compatibility, and long-term performance for the exact polymer grade.
Composite panels aligned for structural adhesive bonding
Composite bonding
Suitable for evaluation in composite-bonding applications requiring controlled adhesive thickness and room-temperature or accelerated cure. Confirm compatibility with the exact resin system, surface condition, layup, and joint design.
Next steps

Technical Support

Contact Krayden to discuss substrate preparation, cartridge dispensing, bondline control, mixed-batch sizing, cure scheduling, and the relevance of the typical aluminum lap-shear, T-peel, bulk-property, and environmental-resistance information to your specific assembly.

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers