LOCTITE EA 9330.3

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE EA 9330.3

Main features

  • Thixotropic Application Control
  • 1-Hour 82 deg C Cure
  • 33.8 MPa Aluminum Lap Shear

Product Description

LOCTITE EA 9330.3 AERO is a two-component, room-temperature-curing epoxy paste adhesive formulated with thixotropic, low-slump handling and high peel strength. The 100:33 Part A-to-Part B weight mix provides a 60-minute pot life for a 100 g mass at 25°C. The mixed adhesive is gray with a density of 1.14 g/mL. It reaches handling strength after 24 hours at temperatures above 25°C and develops normal performance after 5–7 days, with an alternative 1-hour cure at 82°C for small masses. Typical testing on phosphoric-acid-anodized 2024-T3 AlClad aluminum demonstrates tensile lap shear and peel performance across subzero, ambient, and elevated temperatures.

Key features

  • Low-slump thixotropic paste: Supports controlled placement before cure without converting the rheology description into a drip- or void-prevention claim.
  • Defined mix and working window: Mix Part A and Part B at 100:33 by weight; typical pot life is 60 minutes at 25°C for a 100 g mass.
  • Room-temperature or accelerated cure: Normal performance develops after 5–7 days above 25°C; a 1-hour cure at 82°C may be used for small mixed masses.
  • Prepared-aluminum lap shear performance: Typical tensile lap shear is 33.8 MPa at 25°C after a 5-day room-temperature cure on phosphoric-acid-anodized 2024-T3 AlClad aluminum.
  • Peel performance: Typical floating roller peel is 414 N/25 mm at 25°C after a 5-day room-temperature cure under the stated test conditions.

Technical Specifications

General Properties
Color
The color
Gray (Part A) / Clear (Part B) / Gray (Mixed)
Density (g)
1.17 (Part A) / 1.06 (Part B) g/cm3
Mix Ratio
The amount of a constituent divided by the total amount of all other constituents in a mixture
100:33 by weight
Physical Properties
Viscosity (Part A)
120,000 to 500,000 mPa.s
Viscosity (Part B)
22,000 to 48,400 mPa.s

Additional Information

Aerospace epoxy adhesive

LOCTITE EA 9330.3 AERO

LOCTITE EA 9330.3 AERO is a two-component, thixotropic epoxy paste adhesive developed for low-slump application and high peel strength. It mixes at 100:33 by weight, provides a 60-minute pot life at 25°C for a 100 g mass, and supports room-temperature cure or an accelerated 1-hour cure at 82°C for small mixed quantities.

Two-component epoxy paste Thixotropic low-slump 100:33 mix ratio by weight 60-minute pot life at 25°C Room-temperature cure High peel strength
LOCTITE EA 9330.3 AERO product image

LOCTITE EA 9330.3 AERO

As-Supplied Properties

Mix ratio
100:33 by weight
Part A to Part B. Volume measurement is not recommended for structural applications unless ratio control is assured.
Pot life
60 minutes
Typical for a 100 g mass at 25°C using ASTM D2471 in a water bath.
Mixed state
Gray thixotropic paste
Mixed density is 1.14 g/mL; low-slump behavior supports placement control before cure.
Property Value Unit / state Method / condition
Color Gray / clear / gray Part A / Part B / mixed As supplied and immediately after complete mixing
Part A viscosity 120–550 Pa·s 25°C; Brookfield HBT, spindle 7 at 2.1 rad/s
Part B viscosity 22.0–48.4 Pa·s 25°C; Brookfield HBT, spindle 5 at 2.1 rad/s
Part A density 1.17 g/mL As supplied
Part B density 1.06 g/mL As supplied
Mixed density 1.14 g/mL After mixing at the specified ratio
Part A warranty life 1 year Stored below 25°C
Part B warranty life 1 year Stored below 25°C
Preparation and bonding

Processing and Cure

Bring the separate components close to room temperature, then combine and mix completely at the specified weight ratio. Do not mix quantities greater than 250 g because heat buildup can cause uncontrolled decomposition and toxic fumes. Apply the adhesive to clean, dry, properly prepared bonding surfaces and hold the parts in contact until set. Remove uncured excess before it hardens; denatured alcohol and many common industrial solvents may be suitable when used in accordance with the solvent supplier’s safety instructions.

Mix ratio: 100 parts Part A to 33 parts Part B by weight.
Pot life: Typical 60 minutes at 25°C for a 100 g mixed mass, ASTM D2471 in a water bath.
Handling strength: 24 hours above 25°C; support tooling or pressure may then be removed, but loading should remain limited because full bond strength has not yet developed.
Cure schedules: 5–7 days above 25°C for normal performance. For small mixed masses, accelerated cures up to 93°C may be used; 1 hour at 82°C provides complete cure.
Storage and Handling

Keep each component tightly closed in a cool, well-ventilated area away from incompatible materials. Warranty life is 1 year for both Part A and Part B when stored below 25°C. Do not heat Part B above 100°C. Use adequate ventilation, avoid skin and eye contact, and follow current product labeling and safety documentation before use.

Final material state

Cured Properties

Typical bulk-resin properties under the stated specimen, temperature, frequency, and test-method conditions.

Property Typical value Unit Method / condition
Tensile strength 42.0 MPa 25°C; ASTM D638 using 3.18 mm castings
Tensile modulus 2687 MPa 25°C; ASTM D638 using 3.18 mm castings
Elongation at break 9 % 25°C; ASTM D638 using 3.18 mm castings
Shore D hardness 81 Shore D 25°C
Glass transition temperature 54 °C DMTA
Cured density 1.11 g/cm³ ASTM D1622
Dielectric constant 4.46 — 1 kHz and 25°C; ASTM D150
Dissipation factor 0.013 — 1 kHz and 25°C; ASTM D150

Performance Evidence

The following typical results preserve the tested substrate, surface preparation, cure, bondline, method, and temperature conditions needed for technical interpretation.

Tensile lap shear across test temperatures
Typical tensile lap shear decreases with increasing test temperature while remaining above the defined 6.9 MPa service-temperature threshold at 82°C.
Test temperature Typical strength (MPa) Typical strength (psi)
−55°C 39.3 5,700
25°C 33.8 4,900
71°C 11.7 1,700
82°C 7.6 1,100
ASTM D1002; 2024-T3 AlClad aluminum treated by phosphoric acid anodizing per ASTM D3933; cured 5 days at 25°C. Service temperature is defined as the temperature at which the adhesive retains 6.9 MPa tensile lap shear and is 82°C.
Bondline thickness effect at 25°C
Typical tensile lap shear values were measured across bondlines from 0.08 to 1.91 mm under the same prepared-aluminum configuration.
Bondline thickness Typical strength (MPa) Typical strength (psi)
0.08 mm 35.8 5,200
0.13 mm 34.5 5,000
0.25 mm 33.1 4,800
1.27 mm 28.9 4,200
1.91 mm 26.2 3,800
Tested at 25°C after curing 5 days at 25°C on phosphoric-acid-anodized 2024-T3 AlClad aluminum. Results are configuration-specific typical values, not universal joint design allowables.
Post-cure exposure at 71°C
After an initial 5-day cure at 25°C, specimens were post-cured at 71°C for the listed durations and tested at 25°C and 71°C.
Post-cure duration Tested at 25°C (MPa) Tested at 71°C (MPa)
3 days 37.2 15.8
7 days 41.3 14.5
15 days 42.0 15.2
30 days 42.7 16.5
60 days 41.3 14.5
ASTM D1002 prepared-aluminum configuration. Post-cure duration and test temperature must remain attached to each result.
T-peel performance by bondline thickness
Typical T-peel values were measured at 25°C across bondline thicknesses from 0.08 to 0.76 mm.
Bondline thickness Typical T-peel (N/25 mm) Typical T-peel (lb/in)
0.08 mm 223 50
0.13 mm 223 50
0.25 mm 245 55
0.50 mm 267 60
0.76 mm 258 58
ASTM D1876; 2024-T3 AlClad aluminum treated by phosphoric acid anodizing per ASTM D3933; cured 5 days at 25°C.
Peel-rate and floating-roller peel results
T-peel remained 200 N/25 mm at the evaluated peel rates, while floating-roller peel varied with test temperature.
T-peel rate Typical T-peel
51 mm/min 200 N/25 mm
127 mm/min 200 N/25 mm
254 mm/min 200 N/25 mm
305 mm/min 200 N/25 mm
762 mm/min 200 N/25 mm
Floating-roller test temperature Typical peel (N/25 mm) Typical peel (lb/in)
−55°C 129 29
25°C 414 93
70°C 53 12
T-peel tested per ASTM D1876; floating-roller peel tested per ASTM D3167. Both used specimens cured 5 days at 25°C.
Next steps

Technical Support

Contact Krayden to discuss mix control, surface preparation, bondline selection, cure scheduling, and the relevance of the typical lap-shear and peel data to your specific substrates, joint geometry, production process, and operating temperatures.

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers