LOCTITE EA 9323

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE EA 9323

Main features

  • Low-Viscosity Adhesive Application
  • 30-Minute Working Window
  • 5-Day Cure Cycle

Product Description

LOCTITE EA 9323 AERO is a two-component, low-viscosity epoxy paste adhesive for room-temperature repair of metal and composite aerospace structures. The unfilled amber system supports laminating and injection processes and combines a 30-minute pot life at 25°C for a 450 g mass with handling strength after 24 hours and full room-temperature cure in 5 to 7 days. Typical tensile lap shear reaches 28.9 MPa at 25°C on phosphoric-acid-anodized 2024-T3 AlClad aluminum after a 5-day cure. The adhesive also retains 7.6 MPa at 121°C under the same ASTM D1002 configuration, providing high-temperature strength data for application evaluation.

Key features

  • Two-component epoxy paste: Amber Part A and Part B form an unfilled structural adhesive system.
  • Low-viscosity components: Part A is 170 Pa·s and Part B is 2.0 Pa·s at 25°C under their stated Brookfield conditions.
  • Controlled mixing: Mix Part A and Part B at 100:45 by weight.
  • Defined working window: Typical pot life is 30 minutes at 25°C for a 450 g mass.
  • Room-temperature or accelerated cure: Cure for 5 to 7 days above 25°C, or use the supported small-mass accelerated schedule.

Suitable for

  • Repair of metal aerospace structures
  • Repair of composite aerospace structures
  • Laminating and adhesive-injection repair processes

Technical Specifications

General Properties
Color
The color
Amber
Density (g)
1.17 (Part A) / 0.96 (Part B) g/cm3
Mix Ratio
The amount of a constituent divided by the total amount of all other constituents in a mixture
100:45 by weight
Physical Properties
Viscosity (Part A)
170,000 mPa.s
Viscosity (Part B)
2000 mPa.s

Additional Information

Aerospace structural adhesive

LOCTITE EA 9323 AERO

This two-component, low-viscosity epoxy paste adhesive cures at room temperature for repair of metal and composite structures. Its unfilled formulation is used in laminating and injection processes, with supported lap-shear performance from -55°C to 177°C under the stated aluminum test configuration.

Two-component epoxy Low-viscosity paste Room-temperature cure Unfilled formulation High-temperature strength
LOCTITE EA 9323 AERO two-component epoxy adhesive packaging

Two-part LOCTITE EA 9323 AERO adhesive system

As supplied

As-Supplied Properties

Typical component properties and the required bulk-mixing ratio. Viscosity values apply to the separate components under the stated conditions.

Property Value Unit Method / condition
Product form Two-component epoxy paste adhesive — Unfilled Part A and Part B system mixed immediately before application.
Color Amber — Part A, Part B, and mixed adhesive.
Part A viscosity 170 Pa·s 25°C; Brookfield HBT, spindle 5 at 10 rpm.
Part B viscosity 2.0 Pa·s 25°C; equivalent to 20 Poise; Brookfield HBT, spindle 1 at 20 rpm.
Mix ratio, Part A:Part B 100:45 by weight Volume measurement is not recommended for structural applications unless special precautions assure the correct ratio.
Processing

Mixing, Application, and Cure

Bring the separate components close to room temperature, combine them at the required weight ratio, and mix completely before applying to clean, dry, prepared bonding surfaces. Control mixed mass and cure conditions to manage the working window and exotherm.

Mix ratio: 100 parts Part A to 45 parts Part B by weight.
Pot life: 30 minutes at 25°C for a 450 g mass, ASTM D2471 in a water bath.
Handling strength: 24 hours above 25°C; keep initial loads small because full bond strength has not yet developed.
Cure: 5 to 7 days above 25°C for normal performance; for small masses, 1 hour at 82°C provides complete cure, with accelerated cures permitted up to 93°C.

Recommended Processing Sequence

Stage 1
Prepare the surfaces
Make sure bonding surfaces are clean, dry, and properly prepared before adhesive application.
Stage 2
Proportion and mix
Combine Part A and Part B at 100:45 by weight and mix thoroughly. Do not mix more than 450 g because heat buildup may cause uncontrolled decomposition and toxic fumes.
Stage 3
Apply and hold
Apply the mixed adhesive and hold the bonded parts in contact until the adhesive is set. Support tooling or pressure may be removed after handling strength develops.
Stage 4
Cure and clean up
Follow the selected cure schedule and remove excess uncured adhesive from tools and the work area before it hardens. Use solvents only in accordance with the solvent supplier's safety information.
Storage and Handling

Store both components between 0°C and 25°C in tightly closed containers in a cool, well-ventilated area. At temperatures below 4°C, shelf life is 1 year for Part A and Part B. At temperatures below 25°C, shelf life is 3 months for Part A and 1 year for Part B. Place the material into its intended storage condition promptly after receipt.

After cure

Cured Material Properties

Typical bulk-resin and electrical properties. These values describe prepared test specimens and should not be treated as guaranteed design allowables for every bonded assembly.

Property Typical value Unit Method / condition
Service temperature 121 °C Defined as the temperature at which the adhesive retains 6.9 MPa by ASTM D1002.
Tensile strength 24.1 MPa 25°C; ASTM D638 using 3.18 mm castings.
Tensile modulus 2.58 GPa 25°C; ASTM D638 using 3.18 mm castings.
Elongation at break 9.0 % 25°C; ASTM D638 using 3.18 mm castings.
Shore D hardness 84 — 25°C.
Glass transition temperature, dry 97 °C Bulk-resin property.
Glass transition temperature, wet 69 °C Bulk-resin property.
Shear modulus 930 MPa Bulk-resin property.
Poisson's ratio 0.39 — Bulk-resin property.
Compressive strength 60.6 MPa 25°C; ASTM D695 using 12.7 mm castings.
Compressive modulus 1.833 GPa 25°C; ASTM D695 using 12.7 mm castings.
Dielectric constant 3.43 — 1 kHz at 25°C; electrical properties tested per ASTM D149/D150.
Dissipation factor 0.017 — 1 kHz at 25°C; electrical properties tested per ASTM D149/D150.

Bond Strength Performance

The following typical results preserve the tested substrates, surface preparations, cure, exposure, and test temperatures. Bond strength in another assembly depends on its materials, joint geometry, preparation, cure, and service conditions.

Tensile lap shear across test temperature
Test temperature Typical lap shear, MPa
-55°C 19.3
25°C 28.9
82°C 8.3
121°C 7.6
177°C 4.1
ASTM D1002 after 5 days at 25°C; 2024-T3 AlClad aluminum, phosphoric-acid anodized per ASTM D3933.
Tensile lap shear after environmental exposure
Exposure before test Typical lap shear, MPa
Control 28.9
49°C / 100% RH / 30 days 19.3
Salt spray at 41°C / 30 days 21.7
ASTM D1002 test at 25°C after the stated exposure; same aluminum preparation and 5-day cure as the control.
Floating-roller peel strength
Test temperature Typical peel strength, N/25 mm
-55°C 22
25°C 18
82°C 98
ASTM D3167 after 5 days at 25°C; 2024-T3 bare aluminum treated with FPL etch per ASTM D2651.
Application contexts

Applications

LOCTITE EA 9323 AERO is used for repair work where its room-temperature cure, low component viscosity, and tested metal-bond performance align with the selected structure, preparation, and cure process.

Metal aerospace structure repair with epoxy adhesive applied to a prepared joint
Metal structure repair
Room-temperature cure and the aluminum lap-shear dataset support evaluation for repair of properly prepared metal structures.
Composite aerospace panel repair with adhesive positioned in the damaged area
Composite structure repair
The adhesive is used for composite-structure repair when the material set, surface preparation, joint design, and cure process are validated for the assembly.
Technician performing controlled adhesive injection or laminating repair on an aerospace structure
Laminating and injection
The low-viscosity, unfilled system is used in laminating and adhesive-injection repair processes with controlled mixing, application, and cure.
Next steps

Technical Support for LOCTITE EA 9323 AERO

Krayden can help review mix ratio, batch size, cure schedule, surface preparation, and the test conditions that matter for a metal or composite repair. Contact our technical team to discuss application fit and processing requirements for LOCTITE EA 9323 AERO.

Leading Brands Trust in Our Products and Services