LOCTITE EA 901NA-B1

Harmonization Code : 5906100000 | Adhesive tape of a width not exceeding 20cm

LOCTITE EA 901NA-B1

Main features

  • Thixotropic Gap-Filling Control
  • 50-Minute Working Window
  • Room-Temperature Application Cure

Product Description

LOCTITE EA 901NA-B1 is a two-component, room-temperature-curing epoxy paste adhesive for bonding metals, rubber, plastics, wood and glass. The gray Part A and amber Part B change to red during thorough mixing, providing a visible mixing indicator. Its thixotropic, sag-resistant paste consistency supports controlled placement and gap filling on bonding surfaces. A 100:23 mix ratio by weight provides a 50-minute pot life for a 450 g mass at 25°C. Assemblies reach handling strength in 8 hours at 25°C, with full cure available through a five-day room-temperature schedule or an accelerated one-hour cure at 93°C. Fully cured bonds resist water, salt spray and most organic liquids.

Key features

  • Thixotropic epoxy paste: Sag-resistant rheology helps the mixed adhesive remain in place and supports gap filling.
  • Visible mixing indicator: Gray and amber components change to red as the two parts are thoroughly mixed.
  • Controlled working window: Typical pot life is 50 minutes for a 450 g mass at 25°C.
  • Flexible cure options: Cure for five days at 25°C or accelerate cure with one hour at 93°C.
  • Environmental exposure resistance: Fully cured bonds resist water, salt spray and most organic liquids.

Applications / Suitable for

  • Bonding prepared metal substrates, including aluminum and steel
  • Plastic-to-metal and engineering-plastic bonding
  • Bonding rubber, wood and glass where the joint design and surface preparation are validated

Technical Specifications

Physical Properties
Viscosity (Part A)
530,000 mPa.s
Viscosity (Part B)
30,000 mPa.s
General Properties
Color
The color
Gray (Part A)/ Amber (Part B) / Red (Mixed)

Additional Information

Aerospace structural adhesive

LOCTITE EA 901NA-B1

This two-component, thixotropic epoxy paste adhesive bonds metals, rubber, plastics, wood and glass. It cures at room temperature, changes from gray and amber components to red during thorough mixing, and provides sag-resistant placement on bonding surfaces. The system supports gap filling and reaches handling strength in 8 hours at 25°C, with room-temperature and accelerated heat-cure options.

Two-component epoxy paste Room-temperature cure Thixotropic and sag resistant Red mix-color indicator 50-minute pot life at 25°C Gap-filling paste
LOCTITE EA 901NA-B1 two-component epoxy paste adhesive packaging

LOCTITE EA 901NA-B1 two-component adhesive system.

As-supplied component properties

Part A viscosity
530 Pa·s
Brookfield HBT, spindle 7 at 2.09 rad/s and 25°C.
Part B viscosity
3.0 Pa·s
Brookfield HBT, spindle 1 at 2.09 rad/s and 25°C.
Property Value Unit Method / condition
Part A color Gray - As supplied
Part B color Amber - As supplied
Part A viscosity 530 Pa·s Brookfield HBT, spindle 7 at 2.09 rad/s, 25°C
Part B viscosity 3.0 Pa·s Brookfield HBT, spindle 1 at 2.09 rad/s, 25°C
Part A shelf life 1 year Store below 4°C (40°F)
Part B shelf life 1 year Store below 4°C (40°F)
Preparation and bonding

Mixing, application and cure

Bring both components close to room temperature, mix at the specified weight ratio, and apply to clean, dry, properly prepared surfaces. Control mixed batch size because the reaction generates heat.

Mix ratio: 100 parts Part A to 23 parts Part B by weight. Volume measurement is not recommended for structural applications unless the ratio is controlled with special precautions.
Pot life: 50 minutes for a 450 g mass at 25°C, ASTM D2471 in a water bath.
Handling strength: 8 hours at 25°C. Support tooling or pressure may then be removed, but load should remain limited until full cure develops.
Cure options: Five days at 25°C for normal performance, or one hour at 93°C for complete cure. Accelerated cures up to 149°C may be used for small masses.
Mixed batch limit: Do not mix quantities greater than 250 g. Excessive heat buildup can cause uncontrolled decomposition and toxic fumes.

Bonding sequence

1
Prepare components and surfaces
Bring Parts A and B close to 25°C. Clean, dry and properly prepare the bonding surfaces before mixing.
2
Mix and apply
Combine the components at 100:23 by weight and mix thoroughly until the system is uniformly red. Apply the mixed paste and assemble the parts within the available pot life.
3
Hold, cure and clean up
Hold the parts in contact until the adhesive has set. Select the room-temperature or accelerated cure schedule, and remove excess uncured adhesive from equipment and work areas before it hardens.
Storage and Handling

Store both components below 4°C (40°F) for a one-year shelf life. Ambient shipment does not alter the standard warranty when the material is placed into its intended storage upon receipt. Use adequate ventilation, avoid skin and eye contact, and review the current component labels and safety information before handling.

Cured bulk material properties

Tensile strength
29.6 MPa
Typical bulk result at 25°C using ASTM D638 castings.
Compressive strength
122.6 MPa
Typical ASTM D695 result after a 24-hour cure at 25°C.
Property Value Unit Method / condition
Tensile strength 29.6 MPa ASTM D638; 3.18 mm castings; tested at 25°C
Tensile modulus 540 ksi (approximately 3.72 GPa) - ASTM D638; 3.18 mm castings; tested at 25°C
Elongation at break 0.9 % ASTM D638; 3.18 mm castings; tested at 25°C
Shore D hardness 90 - Tested at 25°C
Compressive strength 122.6 MPa ASTM D695; 12.7 mm castings; cured 24 hours at 25°C and tested at 25°C
Bond performance

Typical tensile lap-shear strength by cure and test temperature

Typical laboratory results for phosphoric-acid-anodized 2024-T3 Alclad aluminum. Values are specific to the stated substrate, surface preparation, cure schedule, test temperature and ASTM D1002 configuration.

Property Value Unit Method / condition
Tensile lap shear at -55°C 12.4 MPa ASTM D1002; cured 24 hours at 25°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear at -55°C 23.4 MPa ASTM D1002; cured 1 hour at 93°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear at 25°C 19.3 MPa ASTM D1002; cured 24 hours at 25°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear at 25°C 24.1 MPa ASTM D1002; cured 1 hour at 93°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear at 66°C 7.6 MPa ASTM D1002; cured 24 hours at 25°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear at 66°C 23.4 MPa ASTM D1002; cured 1 hour at 93°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear at 93°C 4.8 MPa ASTM D1002; cured 24 hours at 25°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear at 93°C 17.2 MPa ASTM D1002; cured 1 hour at 93°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933
Tensile lap shear at 121°C 4.8 MPa ASTM D1002; cured 1 hour at 93°C; 2024-T3 Alclad aluminum, phosphoric-acid anodized per ASTM D3933

Additional performance evidence

Environmental, substrate and temperature results support product evaluation when the complete test configuration is considered.

Fluid and salt-spray exposure
Water: 21.4 MPa after 30 days at 25°C. Fire-retardant hydraulic fluid: 21.4 MPa; hydraulic oil: 20.7 MPa; JP-4 fuel: 21.4 MPa; hydrocarbon fluid: 20.7 MPa; and anti-icing fluid: 22.7 MPa after seven days at 25°C. Salt spray: 17.2 MPa after 30 days at 41°C.
Typical lap-shear results after a two-hour cure at 93°C and testing at 25°C.
Substrate-specific examples
ABS plastic bonded to steel reached 4.8 MPa after three days at 25°C. Sandblasted steel reached 23.4 MPa after five days at 25°C and 22.7 MPa after two hours at 77°C.
Values apply only to the stated substrate, preparation, cure and test configuration.
Defined service temperature
107°C (225°F), defined as the temperature at which the adhesive retains 6.9 MPa (1,000 psi) in ASTM D1002 testing after a 93°C cure.
This definition is test-specific and is not an unrestricted continuous-use rating.
Application fit

Bonding applications and substrate contexts

Evaluate the adhesive with the intended substrate grade, surface preparation, joint design, cure schedule and service exposure.

Prepared aluminum and steel bonding with LOCTITE EA 901NA-B1
Prepared metal bonding
Suitable for evaluation on prepared metal substrates. Performance data are available for phosphoric-acid-anodized 2024-T3 Alclad aluminum and sandblasted steel.
Plastic-to-metal bonding with LOCTITE EA 901NA-B1
Plastics and mixed-material assemblies
The adhesive bonds plastics and supports plastic-to-metal evaluation. ABS-to-steel lap-shear data demonstrate that results depend on the exact material and preparation.
Rubber, wood and glass bonding with LOCTITE EA 901NA-B1
Rubber, wood and glass
Consider for bonding rubber, wood and glass where the joint geometry, surface condition, cure and operating environment are validated for the application.
Product resource

Aerospace structural adhesive selection guide

Henkel LOCTITE Structural Adhesives Aerospace Product Selection Guide
Explore Henkel's aerospace structural adhesive portfolio, including film and paste adhesives, primers, metal and honeycomb bonding, composite bonding and repair, potting, edge fill and related solutions.
Next steps

Discuss LOCTITE EA 901NA-B1 for your bonding process

Contact Krayden to discuss substrate preparation, mix and cure options, bondline requirements, product availability, and the evaluation conditions most relevant to your aerospace or industrial assembly.

Leading Brands Trust in Our Products and Services