LOCTITE AA 334

Harmonization Code : 3506.10.00.00 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg

LOCTITE AA 334

Main features

  • Permanent Acrylic Bonding
  • Tough Structural Bonding
  • Flexible Cured Adhesive

Product Description

LOCTITE® AA 334™ is a one-component, high-viscosity, activator-cured structural acrylic adhesive designed primarily for securing permanent magnets in electric-motor assemblies. The light-yellow to dark-yellow-brown liquid requires no adhesive mixing and develops tough, durable bonds with strong impact and peel resistance. It can accommodate bond gaps up to 0.5 mm under specified activator conditions and may also be heat-cured or heat-accelerated when surface priming is undesirable.

Key features

  • Permanent-magnet bonding: Designed for securing magnets in motor and other rigid metal assemblies.
  • Tough structural performance: Provides strong lap-shear, impact, and peel resistance in demanding bonded joints.
  • Flexible cure options: Cures with LOCTITE Activator 7387 and can also be accelerated or completed using controlled heat.

Technical Specifications

General Properties
Appearance
Appearance at room temperature.
Light yellow liquid
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.05
Physical Properties
Viscosity
Viscosity is a measurement of a fluid’s resistance to flow. Viscosity is commonly measured in centiPoise (cP). One cP is defined as the viscosity of water and all other viscosities are derived from this base. MPa is another common unit with a 1:1 conversion to cP. A product like honey would have a much higher viscosity -around 10,000 cPs- compared to water. As a result, honey would flow much slower out of a tipped glass than water would. The viscosity of a material can be decreased with an increase in temperature in order to better suit an application
50,000 - 120,000 mPa.s

Additional Information

Technical properties

As-supplied / before-processing properties

Typical uncured and processing properties; cure response depends on activator placement, bond gap, substrate, temperature, assembly time, and optional heat exposure.

Property Value Unit Method / condition
Technology Acrylic — Structural adhesive technology
Chemical type Modified acrylic — Uncured material
Appearance Light yellow to dark yellow-brown liquid — TDS lists light yellow; SDS lists dark yellow to brown
Components One component — Adhesive requires no mixing
Viscosity classification High — TDS classification
Primary cure mechanism Activator — LOCTITE Activator 7387
Secondary cure mechanism Heat — Used to effect or accelerate cure
Specific gravity 1.05 — At 25°C; TDS
Density 1.05 g/cm³ At 20°C; SDS
Particle size ≤254 µm TDS value
Dynamic viscosity 50,000–120,000 mPa·s Brookfield HBT, 25°C, spindle TB, 20 rpm
Kinematic viscosity 57,000–85,000 mm²/s At 25°C; SDS
Flash point 81.5 °C Pensky-Martens closed cup; SDS
Recommended minimum bond gap 0.05 mm Fixture and lap-shear test condition
Maximum stated bond gap 0.5 mm Activator required on both surfaces; immediate assembly
Fixture time <2 min ISO 4587, steel, 0.05 mm gap, Activator 7387 on one side
Fixture time 15 min ISO 4587, steel, 0.25 mm gap, Activator 7387 on one side
Fixture time 60 min ISO 4587, steel, 0.5 mm gap, Activator 7387 on one side
Heat-cure schedule 121°C / 20 min — Typical bondline heating condition
Heat-cure schedule 149°C / 10 min — Typical bondline heating condition
Heat-cure schedule 177°C / 5 min — Typical bondline heating condition
Technical properties

After-processing / final-state properties

Typical cured properties depend on substrate, activator placement, bond gap, cure time, heat exposure, temperature, and test method.

Property Value Unit Method / condition
Shore hardness 70 Shore D ISO 868
Tensile modulus 1,250 N/mm² ISO 527-2
Tensile strength at break 21 N/mm² ISO 527-2
Lap-shear strength ≥11 N/mm² ISO 4587, steel, 0.05 mm gap, 24 h at 22°C, Activator 7387 on one side
Lap-shear strength ≥3.5 N/mm² ISO 4587, steel, 0.5 mm gap, 24 h at 22°C, Activator 7387 on one side
180° peel strength 4.4 N/mm ISO 8510-2, steel
Hot-strength retention Approx. 75 % initial strength Approximately 50°C; tested hot; chart-derived
Hot-strength retention Approx. 48 % initial strength Approximately 100°C; tested hot; chart-derived
Hot-strength retention Approx. 18 % initial strength Approximately 150°C; tested hot; chart-derived
Heat-aging retention 110 % initial strength 1,000 h at 90°C; tested at 22°C
Heat-aging retention 100 % initial strength 1,000 h at 120°C; tested at 22°C
Heat-aging retention 105 % initial strength 1,000 h at 150°C; tested at 22°C
Heat-aging retention 100 % initial strength 1,000 h at 175°C; tested at 22°C
Heat-aging retention 10 % initial strength 1,000 h at 200°C; tested at 22°C
Water/glycol resistance 110 % initial strength 50/50 water/glycol, 87°C, 720 h; tested at 22°C
Unleaded-gasoline resistance 15 % initial strength 87°C, 720 h; tested at 22°C
Motor-oil resistance 110 % initial strength 87°C, 720 h; tested at 22°C
Automatic-transmission-fluid resistance 90 % initial strength 87°C, 720 h; tested at 22°C
Brake-fluid resistance 0 % initial strength 87°C, 720 h; tested at 22°C

Leading Brands Trust in Our Products and Services