LOCTITE AA 3035

Harmonization Code : 3506.10.00.00 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg

LOCTITE AA 3035

Main features

  • Low Energy Plastic Bonding
  • Fast Room-Temperature Bonding Cure
  • Multi-Substrate Durability Acrylic Bonding

Product Description

LOCTITE® AA 3035™ is a two-component, room-temperature-curing acrylic adhesive designed for high-strength bonding of low-surface-energy plastics without surface pretreatment. The 1:1 mix-ratio system forms tough, durable bonds on substrates including HDPE and polypropylene and can also bond metals, glass, epoxy, ABS, PVC, and polycarbonate. It provides a seven-minute working time, rapid fixture on HDPE, low odor, and strong resistance to humidity, water, motor oil, water/glycol, diesel exhaust fluid, dilute sulfuric acid, and ammonia.

Key features

  • Low-energy plastic bonding: Bonds HDPE and polypropylene without surface pretreatment.
  • Fast room-temperature cure: Provides approximately seven minutes of working time and fixtures HDPE in less than 20 minutes.
  • Multi-substrate durability: Develops tough bonds to plastics, metals, glass, and epoxy with resistance to demanding environmental exposures.

Technical Specifications

General Properties
Appearance
Appearance at room temperature.
Transparent clear to amber gel
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
0.99
Physical Properties
Viscosity
Viscosity is a measurement of a fluid’s resistance to flow. Viscosity is commonly measured in centiPoise (cP). One cP is defined as the viscosity of water and all other viscosities are derived from this base. MPa is another common unit with a 1:1 conversion to cP. A product like honey would have a much higher viscosity -around 10,000 cPs- compared to water. As a result, honey would flow much slower out of a tipped glass than water would. The viscosity of a material can be decreased with an increase in temperature in order to better suit an application
4,000 - 11,000 mPa.s

Additional Information

Technical properties

As-supplied / before-processing properties

Typical uncured and mixed-material properties; values are reference data rather than guaranteed product specifications.

Property Value Unit Method / condition
Technology Acrylic — Two-component adhesive system
Chemical type Methacrylate — Uncured components
Component A appearance Transparent clear to amber gel — Resin
Component B appearance Transparent clear to amber gel — Hardener
Mixed appearance Pale yellow — After mixing Parts A and B
Components Two component — Requires mixing
Mix ratio 1:1 by volume Part A : Part B
Cure mechanism Room-temperature cure — Two-part acrylic reaction
Part A specific gravity 0.99 — At 25°C
Part B specific gravity 0.99 — At 25°C
Mixed specific gravity 0.99 — At 25°C
Part A dynamic viscosity 4,000–11,000 mPa·s Cone and plate, 25°C; CP50-1, shear rate 20 s−1
Part B dynamic viscosity 40,000–80,000 mPa·s Cone and plate, 25°C; CP50-1, shear rate 20 s−1
Working time 7 min At 25°C on steel, aluminum, or polyethylene
Fixture time <20 min ISO 4587; HDPE; time to reach 0.1 N/mm² shear strength
Fixture time 10–15 min ISO 4587; HDPE to steel
Peak exotherm temperature 31 °C 10 g mixed mass; peak reached after more than 60 minutes
Part A density 0.9969 g/cm³ Current SDS value; method not stated
Part A flash point 82.5 °C Pensky-Martens closed cup; current SDS
Technical properties

After-processing / final-state properties

Typical cured-material properties depend on substrate, surface preparation, bond geometry, cure time, temperature, and test method.

Property Value Unit Method / condition
Impact strength 5.8 J ISO 9653; HDPE; tested at 21°C after 72-hour cure at 21°C
Impact strength 3.2 J ISO 9653; HDPE; tested at 100°C
Impact strength 6.1 J ISO 9653; HDPE; tested at −40°C
T-peel strength 8 N/mm ISO 11339; steel
T-peel strength 2 N/mm ISO 11339; aluminum
Block shear strength ≥6.9 N/mm² ISO 13445; HDPE; cured 72 hours at 21°C
Block shear strength 4.5 N/mm² ISO 13445; polypropylene
Block shear strength 14 N/mm² ISO 13445; epoxy
Block shear strength 3 N/mm² ISO 13445; ABS
Block shear strength 8 N/mm² ISO 13445; PVC
Block shear strength 4.5 N/mm² ISO 13445; polycarbonate
Block shear strength 5.8 N/mm² Glass; substrate failure reported
Block shear strength 5.2 N/mm² HDPE to glass; substrate failure reported
Block shear strength 5.8 N/mm² Steel to glass; substrate failure reported
Lap-shear strength 2.5 N/mm² ISO 4587; grit-blasted mild steel
Lap-shear strength 2.5 N/mm² ISO 4587; aluminum
Motor-oil resistance 90 % initial strength 10W30 motor oil at 22°C; 1,000-hour exposure
Water/glycol resistance 115 % initial strength 50/50 water/glycol at 22°C; 1,000-hour exposure
DEF resistance 145 % initial strength AdBlue-type diesel exhaust fluid at 22°C; 1,000-hour exposure
10% sulfuric-acid resistance 105 % initial strength At 22°C; 1,000-hour exposure
Ammonia resistance 110 % initial strength At 22°C; 1,000-hour exposure