Hysol GR30 | Black Epoxy Mold Compound

Harmonization Code : 3907.30.00.85 | Polyacetals, other polyethers and epoxide resins, in primary forms; polycarbonates, alkyd resins, polyallyl esters and other polyesters, in primary forms : Epoxide resins : Other

Hysol GR30 | Black Epoxy Mold Compound

Main features

  • Designed for TO220 & TO247
  • Improved version of GR300
  • Faster cycle time for Automold

Product Description

Hysol GR30 is a halogen-free, black, semiconductor-grade epoxy molding compound or duroplast designed for the encapsulation and protection of TO220 and TO247 power devices. Once molded and post-mold cured, this product provides optimium protection and reliability for these semiconductor devices. It is a more productive version of GR300 with a CTI of 600V. While GR300 is a great product for TO220 and TO247 it is not as productive as other EMC products. The number of shots that can be done is less than some other EMC and depending on the age of the mold, the GR300 can sometimes stick in the mold making it more difficult to get the parts out. Furthermore, GR300 was designed to be used in multi-gang pot (MGP) molds and conventional molds where the cure time does not need to be fast. GR30 has a shorter gel time, giving it a faster cycle time for automold equipment.

Hysol GR30 was formulated to have better electrical properties then its predecessor. This means that the GR30 passes higher levels of high-temperature reverse bias (HTRB) than the standard GR300 and offers excellent HTRB performance. Additionally, it is an environmentally "Green" product, meaning that it doesn't contain any bromine, antimony or phosphorus flame retardants. Previous MG-series EMC dominated the space for power semiconductors but used halogen-containing flame retardants. This next generation epoxy mold compound replaces these older generation products. It is designed to achieve JEDEC Level 1 requirements at 260°C reflow temperature on Nickel or Nickel-plated leadframes. And to top that up, it meets UL 94 V-0 Flammability at 1/8 inch (3.18mm) thickness. This product is an alternative that can easily replace the discontinued Kyocera KE-G300S.

Available Versions: 

  • GR350HT (High Thermal Conductivity of 1.95 W/mK)

Key Features

  • Low thermal stress and excellent electrical stability.
  • Excellent reliability performance on TC, PCT, etc.
  • Meet with all type devices especially MOSFET, Schottky, etc.
  • Good delam performance after stress test
  • Good adhesion performance
  • Excellent workability - 500 shots continuous molding
  • Suitable for Conventional/MGP/Auto Mold type
  • Green material without Br/Sb in compliance with ROHS.
  • Meet UL94 V-0 flammability rate at 1/8 inch thickness.

Key Features for Rotor Magnet Fixing

  • Good filling ability for gap around magnets in rotor.
  • Good binding force for rotor and magnet.
  • Excellent reliability performance at working temperature. 
  • Fast cure for high effective units per hour.

 

 

Product Family

HYSOL GR30

1. Select Product Form
2. Select Pellet Size
3. Select Pellet Weight
4. Select Package Size

Loading pricing…

Product availability
US Shipping in 12 weeks
CA Shipping in 12 weeks
EU Shipping in 12 weeks
Packaging
Please select Product Form, Pellet Size, Pellet Weight and Package Size.
TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color
The color
Black
Filler Content
80 %
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.94
Thermal Properties
Glass Transition Temperature (Tg)
The glass transition temperature for organic adhesives is a temperature region where the polymers change from glassy and brittle to soft and rubbery. Increasing the temperature further continues the softening process as the viscosity drops too. Temperatures between the glass transition temperature and below the decomposition point of the adhesive are the best region for bonding. The glass-transition temperature Tg of a material characterizes the range of temperatures over which this glass transition occurs.
178 °C
Thermal Conductivity
Thermal conductivity describes the ability of a material to conduct heat. It is required by power packages in order to dissipate heat and maintain stable electrical performance. Thermal conductivity units are [W/(m K)] in the SI system and [Btu/(hr ft °F)] in the Imperial system.
1.0 W/m.K
UL 94 Rating
Flammability rating classification. It determines how fast a material burns or extinguishes once it is ignited. HB: slow burning on a horizontal specimen; burning rate less than 76 mm/min for thickness less than 3 mm or burning stops before 100 mm V-2: burning stops within 30 seconds on a vertical specimen; drips of flaming particles are allowed. V-1: burning stops within 30 seconds on a vertical specimen; drips of particles allowed as long as they are not inflamed. V-0: burning stops within 10 seconds on a vertical specimen; drips of particles allowed as long as they are not inflamed. 5VB: burning stops within 60 seconds on a vertical specimen; no drips allowed; plaque specimens may develop a hole. 5VA: burning stops within 60 seconds on a vertical specimen; no drips allowed; plaque specimens may not develop a hole
V0
Electrical Properties
Volume Resistivity
Volume resistivity, also called volume resistance, bulk resistance or bulk resistivity is a thickness dependent measurement of the resistivity of a material perpendicular to the plane of the surface.
11000000000000000 Ohms⋅cm
Mechanical Properties
Molded Shrinkage
0.24 %
Chemical Properties
Moisture absorption
0.42 %
Physical Properties
Spiral Flow @ 175°C
66 cm
Curing Conditions
Transfer Pressure
40 - 100 kg/cm2
Transfer Time
5 - 30 s

Additional Information

Designed for TO220 & TO247 devices

TO220 and TO247 are big, bulky packages, so molding these products with a standard mold compound is fairly easy without using any fine fillers. The trouble with these packages however is that epoxy mold compounds used typically fail Hig Temperature Reverse Bias (HTRB) testing, which exposes the device to humidity and temperature while the device is under BIAS. Devices often experience "gate leakage" under these conditions and fail catastrophically.

Furthermore, these devices are often used using a Nickel (Ni) plated Cu leadframe, which is very difficult to adhere to. Customer reliability testing on TO3P, TO220, and TO252 packages using GR30 has demonstrated excellent adhesion of the EMC to Nickel (Ni) plated Cu leadframe, with minimal to zero delamination observed after testing.  Specifically, GR30 utilized in TO220 packages exhibited no delamination after TCT500 (-65°C to 150°C) and PCT96 tests. For GR30 in TO252 packages, only non-critical delamination was observed after the same TCT500 (-65°C to 150°C) and PCT96 tests.

GR30-ON for Automotive TO247/TO220 

 
Item Unit GR30 GR30-ON
EMC Grade - GR30 GR30-ON
Epoxy resin - EOCN + DCPD EOCN + LSR*
Flame Retardant - Inorganic MH Self Extinguish
Filler shape - Angular & Spherical Angular & Spherical
Filler max sieving size µm 150 150
Filler content wt% 80 ± 1 % 84 ± 1 %
Spiral flow inch 24 27
Gelation time @ 175°C sec 18 25
Flexural strength @ 25°C MPa 110 110
Flexural modulus @ 25°C MPa 15640 17600
Tg °C 175 165
Coefficient of thermal expansion α1 ppm/°C 14 10
Coefficient of thermal expansion α2 ppm/°C 55 38
Thermal conductivity W/m·K 1.0 0.9
Specific gravity g/cm³ 1.94 1.90
Na+ (extracted water) ppm 5 3
Cl- (extracted water) ppm 8 11
pH (extracted water) - 5.2 5.3
Water absorption (PCT) wt% 0.45 0.38
Flammability (UL94) - V-0 V-0

Note:
1. LSR* stands for low stress resin with self extinguish property;
2. GR30-ON is commerical product for TO247/TO220 automotive application;
3. Property data are typical value for reference only, not to be used as quality guarantee

GR30 and GR30-ON are high-performance EOCN-based epoxy molding compounds with optimized filler loading, UL94 V-0 flammability, and a balanced set of mechanical, thermal, and electrical properties for reliable encapsulation. GR30 is well suited for applications that prioritize high Tg and stiffness, while GR30-ON, with its higher spiral flow and lower CTE, is ideal for more complex or stress-sensitive package designs allowing customers to select the grade that best matches their device, process, and reliability requirements.

GR30 Thermal Degradation Performance

GR30_TGA
In an inert atmosphere, Hysol GR30 shows a single dominant degradation event with negligible mass change up to ~300–350 °C, indicating low volatile content and good bake stability. By the extrapolated-tangent method, T₅% = 406 °C and T₁₀% = 434 °C. The DTG trace peaks at Tmax = 430 °C with a maximum rate of 0.00385 %/°C, marking the principal scission of the organic network. Residue at 800 °C is high (char = 82.41 %) with total mass loss = 17.59 %, consistent with a highly filled epoxy system that carbonizes in N₂. Practically, this profile implies minimal outgassing or weight loss through standard package exposures (post-mold cure 170–190 °C, assembly peaks ≤260 °C), and strong retention of integrity under short, high-temperature excursions below ~400 °C.

In a mixed oxidizing atmosphere, the main event shifts and broadens: T₅% = 424 °C, T₁₀% = 466 °C, and the DTG maximum moves to Tmax = 458 °C with a lower peak rate (0.0028 %/°C). The higher Tmax coupled with a reduced final residue (ash = 78.11 % at 800 °C, total mass loss = 21.89 %) reflects early-stage oxidative stabilization (which can delay the peak rate temperature) followed by oxidation of carbonaceous char at higher temperatures, increasing overall mass loss versus N₂. The tailing DTG in the 450–600 °C region captures progressive char burn-off typical for epoxy systems exposed to oxygen.

 

GR30 — Thermogravimetric & Derivative Thermogravimetric Parameters
Parameter Under Pure N₂ Under N₂ + O₂ Notes
Initial Mass 100 % 100 % Normalized baseline
T5% (5 % mass loss) 406 °C 424 °C T5% determined from TGA curve crossing 95 % mass remaining
T10% (10 % mass loss) 434 °C 466 °C T10% corresponds to 90 % remaining mass
Tonset (Extrapolated Tangent) ≈ 405 °C ≈ 420 °C Intercept from first DTG inflection
Tmax (DTG peak) 430 °C @ 0.00385 %/°C 458 °C @ 0.0028 %/°C Tmax = temperature of maximum mass-loss rate
Main Decomposition Range 400–480 °C 420–500 °C Slightly delayed oxidation due to oxidative stabilization lag
Total Mass Loss (to 800 °C) 17.59 % 21.89 % More oxidative degradation in mixed gas
Char/Ash Yield @ 800 °C 82.41 % (char residue) 78.11 % (oxidized ash) Indicates higher carbonization in inert N₂ and greater oxidation under N₂ + O₂



GR30 — Temperature-Dependent Properties
Property Unit 25 °C 150 °C 175 °C
Volume Resistivity Ω·cm 13 0.24 0.1
Flexural Strength  MPa 108 76 57
Flexural Modulus  MPa 16 702 2 273 1 893
Adhesion Strength to Cu (post PMC) N 411 353 354
Adhesion Strength to Cu (post MSL3) N 14 22 8
Adhesion Strength to Cu (post PMC) MPa 7.12 6.11 6.13
Adhesion Strength to Cu (post MSL3) MPa 0.24 0.38 0.14

 

GR30 — Thermal, Ionic, and Electrical Properties
Property Unit GR30
Glass Transition Temperature °C 179
Coefficient of Thermal Expansion α1 ppm/°C 14
Coefficient of Thermal Expansion α2 ppm/°C 54
Ion Content
Chlorine (Cl−) ppm 6
Sodium (Na+) ppm 3
Potassium (K+) ppm 1
Bromine (Br−) ppm 0
Sulfate (SO42−) ppm 10
Dielectric Constant at 1 MHz — 3.97
Electrical Conductivity (oEW) µS/cm 17
Thermal Conductivity W/m·K 1.09



GR30 has been successfully used for Magnet Fixing in Electric Vehicle Rotors


Epoxy molding compound is used to bond the magnet and rotor core by using a transfer molding method. There are several slots that go through the core. The permanent magnets are inserted in the slot and then the mold compound is filled into the gap to bind the magnet and the rotor core together.

The critical function of the material is to have a strong binding force between the magnet and the rotor core while also having a good filling capability. It should also have excellent reliability at working temperature. GR30 is a green material without Br/Sb, in compliance with ROHS that can cure fast for high Units per Hour. 

Molding compounds have already been used in Rotors with Iron as a base material and with rotor working speeds up to 20000rpm and working temperatures up to ±150°C. They pass both Temperature cycling and High temperature ATF resistance tests while retaining 100% of their flexural strength and flexural modulus. This highlights the product's excellent property stability post post-automotive fluid resistance testing.

 

GR30 has excellent Property Stability after Automotive Transmission Fluid(ATF) Resistance Test

GR30 Properties

PROPERTY UNIT GR30
Filler Seiving Cut Size  um 100
Average Filler Size um 21
Filler Content % 80
Specific Gravity  - 1.94
Spiral Flow @175°C cm 66
Hot Plate Gel Time @175°C sec 19
Glass Transition Temperature °C 178

CTE by TMA, α1

CTE by TMA, α2

ppm

ppm

14

54

Thermal Conductivity

W/m·K

1.0

Flexural Strength @25°C

Flexural Modulus @25°C

MPa

Gpa

110

15.6

Mold Shrinkage % 0.24
Flame Retardancy UL-94 V-0
Shelf Life and Storage Condition mon 6 months at 5°C
 

 

Device Information

EMC GR30
Project Condition LVM
Package Type Rotor
Base Material Fe
Rotor Working Speed 20,000 rpm
Working Temperature ≥ 150°C
Mold Model Automold

 

Reliability Test Procedure

ATF Resistance Test Condition
Temperature Cycling 25°C → (155°C for 40hr → -45°C for 8hr) * 4 or 8 cycles → 25°C
High Temperature Test 25°C → 155°C for 1000 hr or 2000 hr (cool down to room temperature every 200 hrs to add ATF) → 25°C

GR30ATFResistanceTest

GR30 Beta Site Reliability Test Results

ATF Resistance Test: Temperature Cycling

Property Property Retention after 16 days
Flexural Strength at RT 100%
Flexural Modulus at RT 100%
Flexural Strength at 260°C 100%
Flexural Modulus at 260°C 100%

 

HYSOL GR30 Z9A vs T36

GR30 Z9A for excellent oil resistance and narrow gap filling (100 µm)

Typical values shown are for reference only and are not product specifications.

GR30 Z9A vs T36 comparison of key material properties
Property Unit GR30 Z9A T36
Technology — Epoxy Epoxy
Appearance — Black Black
Filler Type — Fused & Spherical Silica Fused Silica
Filler Weight % 80 ± 1 80 ± 3
Filler Cut µm 75 75
UL 94 Flammability — V-0 V-0
Spiral Flow @ 175 °C cm 90 106.68
Gel Time @ 175 °C s 20 27
Specific Gravity g/cm³ 1.88 1.88
Glass Transition Temperature (Tg) °C 170 162
Coefficient of Thermal Expansion α1 ppm/°C 11 12
Coefficient of Thermal Expansion α2 ppm/°C 55 54
Flexural Modulus @ 25 °C MPa 15,800 18,300
Flexural Strength @ 25 °C MPa 120 139
Tensile Strength @ 25 °C MPa 80 —
CTI V 600 —
Thermal Conductivity W/m·K 0.8 0.8
Ionic and Electrical Properties
Extractable Chloride (Cl−) ppm 10 12
Extractable Sodium (Na+) ppm 4 7
Moisture Absorption, 24 h PCT % — 0.44
Shrinkage % — 0.31
Volume Resistivity @ 25 °C, 500 V Ω·cm — 12 × 1015
Dielectric Constant @ 1 MHz — — 3.7

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers