EPOCAST 89537

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

EPOCAST 89537

Main features

  • Non-Sag Placement Control
  • Low-Density, Glass-Fiber-Reinforced Syntactic
  • Self-Extinguishing Epoxy Syntactic

Product Description

EPOCAST® 89537 A/B is a two-part, glass-fiber-reinforced epoxy syntactic developed for honeycomb core structures. The low-density, non-sag material can be trowelled or extruded for fastener and attachment potting, core splicing, and edge reinforcement, including vertical applications up to 1/2 inch (1.25 cm) thick. The mixed system forms a gray soft paste with a typical density of 0.90 g/cm³ and a 70-minute gel time for a 100 g mass at 25°C. It is self-extinguishing and meets the requirements of BMS 5-28 Type 32.

Key features

  • Glass-fiber-reinforced syntactic: Two-part, low-density core filler for localized potting, splicing, and reinforcement.
  • Non-sag vertical build: Can be applied vertically at thicknesses up to 1/2 inch (1.25 cm).
  • Self-extinguishing performance: Meets the requirements of BMS 5-28 Type 32.

Applications / Suitable for

  • Fastener and attachment potting in honeycomb core structures
  • Honeycomb core splicing
  • Core-edge reinforcement
  • Vertical or overhead core-filling applications requiring non-sag placement

Technical Specifications

General Properties
Color
The color
Gray
Density (g)
0.9 g/cm3
Mix Ratio
The amount of a constituent divided by the total amount of all other constituents in a mixture
100:18.5

Additional Information

Technical properties

As-supplied / before-processing properties

Typical component and mixed-system properties. Material temperatures should be above 18°C during mixing.

Property Value Unit Method / condition
Appearance A resin: white; B hardener: black; mixed system: gray — Visual
Density A resin: 0.85; B hardener: 1.00; mixed system: 0.90 g/cm³ ASTM D1622; 25°C
A resin viscosity Paste — ASTM D2196; 25°C
B hardener viscosity 10,000 cP ASTM D2196; 25°C
Mixed-system viscosity Soft paste — ASTM D2196; 25°C
Mix ratio 100 : 18.5 Parts by weight A resin : B hardener
Gel time 70 min 100 g mass at 25°C
Technical properties

After-processing / final-state properties

Typical cured properties. Mechanical values below use Cure 1: seven days at 25 ± 1°C.

Property Value Unit Method / condition
Compressive strength 8.50 (58.6) ksi (MPa) ASTM D695; Cure 1
Compressive modulus 450 (3103) ksi (MPa) ASTM D695; Cure 1
Lap shear strength 1,200 (8.3) psi (MPa) ASTM D1002; aluminum-to-aluminum; Cure 1
Weight gain after fluid immersion TT-S-735: 0.40; MIL-M-5606: 0.37; low-density hydraulic fluid: 0.48; distilled water: 0.30 % ASTM D543; 24-hour immersion
Flammability burn rate 1 (2.54) in/min (cm/min) Supplier-reported typical value