EPOCAST 1628

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

EPOCAST 1628

Main features

  • Ultra Low Density Paste
  • Flame-Resistant Application Paste Material
  • Non-Sag Placement Control

Product Description

EPOCAST® 1628 A/B is a two-component, ultra-low-density epoxy syntactic supplied as a soft paste for reinforcing honeycomb structures. The mixed pale-yellow material has a typical density of 0.50 g/cc and an extrudable, non-sag consistency for filling honeycomb core sections and the edges of composite sandwich constructions with a putty knife or trowel. After cure, the material can be sanded and machined for finishing. The flame-retardant system is qualified to BMS 5-28, Type 28, for composite edge-reinforcement applications where lightweight construction and controlled paste placement are important.

Key features

  • Ultra-low-density system: The mixed epoxy syntactic has a typical density of 0.50 g/cc for lightweight honeycomb core and edge reinforcement.
  • Extrudable, non-sag paste: The material can be spread with a putty knife or trowel to fill core sections and composite sandwich edges.
  • Flame-retardant and qualified: Qualified to BMS 5-28, Type 28, with documented FAR 25.853 60-second vertical flammability results.

Applications / Suitable for

  • Edge reinforcing of honeycomb structures
  • Filling honeycomb core sections and edges of composite sandwich constructions

Technical Specifications

General Properties
Color
The color
Pale Yellow
Density (g)
0.50 g/cm3
Mix Ratio
The amount of a constituent divided by the total amount of all other constituents in a mixture
100:25

Additional Information

Technical properties

As-supplied / before-processing properties

Typical values for the separate components and mixed system. These values are not product specifications.

Property Value Unit Method / condition
Color White / yellow / pale yellow — Visual; A resin / B hardener / mixed system
Density 0.45 / 0.52 / 0.50 g/cc ASTM D1622; A resin / B hardener / mixed system
Physical form and rheology Paste — ASTM D2196 at 25°C; A resin, B hardener and mixed system
Mix ratio 100:25 Parts by weight A resin:B hardener; mix thoroughly for several minutes
Gel time 65 min ASTM D2471; 60 g mixed system at 25°C
Typical cure schedule 48 h at 25°C; or gel at room temperature plus 5 h at 52°C — Material should be above 18°C during mixing
Technical properties

After-processing / final-state properties

Typical cured properties for evaluation purposes. Results depend on the stated test method, specimen and temperature and are not product specifications.

Property Value Unit Method / condition
Compressive strength 2,800 (19.3) psi (MPa) ASTM D695 at 25°C
Compressive strength 600 (4.1) psi (MPa) ASTM D695 at 82°C
Compressive strength 550 (3.8) psi (MPa) ASTM D695 at 121°C
Compressive modulus 230 (1.6) ksi (GPa) ASTM D695 at 25°C
Tensile lap shear strength 800 (5.5) psi (MPa) ASTM D1002; aluminum-to-aluminum at 25°C
Vertical flammability 0 s extinguish time; 0.3 in burn length — FAR 25.853; 60-second vertical test
Weight gain after immersion 1.5 / 2.5 / 3.5 / 3.4 % ASTM D543; 24 h at 25°C in Mil-S-3136 Type III fluid / Mil-M-5606 hydraulic fluid / Skydrol 500-A / distilled water, respectively

Leading Brands Trust in Our Products and Services