DOWSIL EG-4131

Harmonization Code : 3907.30.00.40 | Epoxy Mold Compounds containing by weight more than 70 % silicon dioxide

DOWSIL EG-4131

Main features

  • Clear 1:1 Pdms Dielectric Gel
  • 650 cP Mixed Viscosity
  • 91.1% Transmission at 450 Nm

Product Description

DOWSIL EG-4131 Dielectric Gel Kit is a two-part, colorless, flowable PDMS gel that can cure at room temperature or with added heat. It can be used for liquid optical clear coupling in display and LED lighting applications and for coating, encapsulating or potting PCB assemblies where a soft protective gel is required. Documented applications include display optical coupling, led lighting, and pcb coating, encapsulation and potting. The matched-viscosity components can be mixed manually for low-volume work or with static or dynamic meter-mix equipment for higher-volume processes.

Key features

  • Flow and dispensing: Clear 1:1 PDMS gel with 650 cP mixed viscosity for flowable dispensing.
  • Key characteristic: 91.1% transmission at 450 nm through 3.2 mm with a refractive index of 1.41 at 632.8 nm.
  • Processing window: 30-minute working time at 25 C with room-temperature or heat-accelerated cure.

Applications

  • Display optical coupling
  • LED lighting
  • PCB coating, encapsulation and potting

Technical Specifications

General Properties
Appearance
Appearance at room temperature.
Colorless
Component System
Describes the number of components that must be supplied, mixed, or activated before application or cure.
2 Part
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
0.97
Mechanical Properties
Elongation
Elongation is the process of lengthening something. It is a percentage that measures the initial, unstressed, length compared to the length of the material right before it breaks. It is commonly referred to as Ultimate Elongation or Tensile Elongation at break.
175 %
Electrical Properties
Dielectric Strength
Dielectric strength is measured in kV per mm and is calculated by the Breakdown voltage divided by the thickness of the tested material. Those two properties go hand in hand and while Breakdown voltage is always thickness dependent, dielectric strength is a general material property. As an example, the dielectric strength of Polyimide is 236 kV/mm. If we place 1mm of Polyimide between two electrodes, it will act as an insulator until the voltage between the electrodes reaches 236 kV. At this point it will start acting as a good conductor, causing sparks, potential punctures and current flow.
0.54 kV/mm
Volume Resistivity
Volume resistivity, also called volume resistance, bulk resistance or bulk resistivity is a thickness dependent measurement of the resistivity of a material perpendicular to the plane of the surface.
6.32E13 Ohms⋅cm

Additional Information

Potting, Encapsulants & Underfills

Clear 1:1 dielectric gel for optical coupling and electronic protection

DOWSIL EG-4131 Dielectric Gel Kit is a two-part, colorless, flowable PDMS gel that can cure at room temperature or with added heat. It can be used for liquid optical clear coupling in display and LED lighting applications and for coating, encapsulating or potting PCB assemblies where a soft protective gel is required.

1:1 two-part gel650 cP mixed viscosity91.1% at 450 nm30 min pot life

As-Supplied Properties

Flowable 1:1 gel properties

Component and mixed viscosities are separated from cured and optical properties. Values are typical and condition-specific.

Property Typical Value State / Condition
Color Colorless As supplied
Part A viscosity 750 cP (0.75 Pa-s) As supplied
Part B viscosity 650 cP (0.65 Pa-s) As supplied
Mixed viscosity 650 cP (0.65 Pa-s) Mixed
Mix ratio 1:1 Part A : Part B
Working time / pot life 30 minutes 25 deg C

Working time is the time required for the initial mixed viscosity to double at room temperature.

Processing

Meter mixing, de-airing and temperature-controlled cure

The matched-viscosity components can be mixed manually for low-volume work or with static or dynamic meter-mix equipment for higher-volume processes.

  1. Meter Part A and Part B at the 1:1 ratio and mix thoroughly.
  2. Design the mixing and dispensing process to minimize entrapped air.
  3. When needed, vacuum de-air at greater than 28 in. Hg to remove incorporated gas.
  4. Use room-temperature cure or add heat to accelerate the cure reaction.

Tack-free time at 4 mm

  • 80 minutes at 25 deg C.
  • <=10 minutes at 50 deg C.
  • <=5 minutes at 100 deg C.
  • <=5 minutes at 150 deg C.

Allow additional time for the part to heat toward oven temperature and verify the cure schedule in the intended assembly.

Storage and Handling

Keep components dry and tightly closed

Shelf life and storage temperature are identified on the product label. Moisture exposure should be minimized during storage and dispensing.

  • Keep containers tightly closed and minimize headspace.
  • Purge partially filled containers with dry air or nitrogen when needed.
  • Moisture exposure can reduce adhesion and contribute to bubble formation.
  • The product is generally supplied in batch-matched kits containing Part A and Part B.

Technical Guidance

Control air entrapment and cure inhibition

Two process controls are particularly important for addition-cure dielectric gels: minimizing entrained gas and checking materials that may inhibit cure.

Air management

Avoid applying air pressure directly to an exposed liquid gel surface. Bladder packaging, careful mixing and vacuum de-airing can reduce incorporated air before cure.

Compatibility screening

Organotin and other organometallic compounds, sulfur-containing materials, unsaturated hydrocarbon plasticizers and some solder flux residues can inhibit cure. Run a small-scale compatibility test when a material is questionable.

Repair and rework

For PCB assemblies, the gel can be removed to access components. After repair, clean and dry the area before patching with additional silicone gel.

Final-State Properties

Cured, optical and electrical properties

Preserve specimen thickness, wavelength and test configuration when using optical or electrical data.

Property Typical Value Method / Condition
Specific gravity 0.97 Cured
Gel hardness 730 g Cured
Elongation 175% Cured
Unprimed lap shear adhesion 80 psi (0.55 MPa) Glass / glass
Linear CTE 460 ppm/ deg C By DMA
Refractive index 1.41 632.8 nm
Transmission 89.4% / 91.1% / 93.3% 380 / 450 / 760 nm, 3.2 mm
Dielectric strength 13.7 V/mil (0.54 kV/mm) Cured
Volume resistivity 6.32 x 1013ohm-cm Cured

These values are typical and are not specification values.

Applications

Optical coupling and protective gel applications

DOWSIL EG-4131 combines a clear optical path with the soft, resilient behavior of a cured silicone gel.

Display optical coupling

Use as a liquid optically clear coupling material where the refractive index and transmission profile match the assembly requirements.

LED lighting

The product is specifically listed for LED lighting optical-coupling applications.

PCB coating, encapsulation and potting

The gel can be used for coating, encapsulating or potting PCB assemblies, including assemblies with delicate components.

Review optical, cure and dispensing requirements

Krayden can help compare the 1:1 mixing process, optical transmission, refractive index, working time, cure temperature and de-airing requirements of DOWSIL EG-4131 against your display, LED or electronic assembly. Krayden can also help review the documented processing conditions and evaluation criteria before testing.

Contact Us

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers