DEVCON FL-20

Harmonization Code : 3208.20.90 | Paints and varnishes that are dispersed or dissolved in a non aqueous medium

DEVCON FL-20

Main features

  • 30 to 120-Minute Moisture Cure
  • Multi-Substrate Flexane Adhesion Promotion
  • One-Part No-Mix Primer

Product Description

Devcon® FL-20 Primer is a one-part, moisture-cure adhesion-promoting primer used with Devcon® Flexane® products on concrete, wood, rubber, fiberglass, PVC, cured polyurethane, and cured epoxy surfaces. The orange, low-solids primer requires no mixing and provides a 30–120 minute cure time. Depending on the substrate, one or more coats may be applied before top coating with Flexane within the documented application window. Suitability must be evaluated for the intended substrate, preparation method, application, and process conditions.

Key features

  • One-part moisture cure: Requires no mixing and cures in 30–120 minutes under documented conditions.
  • Multi-substrate priming: Intended for concrete, wood, rubber, fiberglass, PVC, cured polyurethane, and cured epoxy.
  • Flexane system compatibility: Conditions applicable surfaces before the application of Devcon® Flexane® products.

Applications / Suitable for

  • Priming concrete and wood before Flexane application
  • Priming gum rubber, neoprene, and cured polyurethane
  • Priming fiberglass, PVC, and cured epoxy surfaces
Product Family

DEVCON FL-20

Loading pricing…

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Color
The color
orange
Solids
3.7 %

Additional Information

Technical properties

As-supplied / before-processing properties

Typical physical and processing properties of Devcon® FL-20 Primer. Typical technical data are not intended for specification purposes.

Property Value Unit Method / condition
Product form One-part moisture-cure primer — Mixing is not applicable
Color Orange — Typical
Solids by volume 3.70 % Typical
Coverage 10 (0.93) per 4 oz ft² (m²) At 5 mils (0.13 mm)
Cure time 30–120 minutes Higher humidity increases cure time
Top-coating window 30–120 minutes Minimum 30 minutes and maximum 2 hours before top coating with Flexane
Storage temperature 70 (21) °F (°C) Store at room temperature

 

Technical properties

After-processing / final-state properties

Typical adhesion results after seven days of cure at 75 °F (24 °C). Results are substrate- and test-configuration-specific and are not intended for specification purposes.

Property Value Unit Method / condition
Adhesion on concrete >50 (>8.8) pli (N/mm) One coat; cured 7 days at 75 °F (24 °C)
Adhesion on cured Flexane >50 (>8.8) pli (N/mm) One coat; cured 7 days at 75 °F (24 °C)
Adhesion on fiberglass >50 (>8.8) pli (N/mm) One coat; cured 7 days at 75 °F (24 °C)
Adhesion on polyester >25 (>4.4) pli (N/mm) One coat; cured 7 days at 75 °F (24 °C)
Adhesion on rubber >50 (>8.8) pli (N/mm) One coat; cured 7 days at 75 °F (24 °C)

Leading Brands Trust in Our Products and Services