CONATHANE TU-701

Harmonization Code : 3910.00.00.90 | Silicones in Primary Forms; Others

CONATHANE TU-701

Main features

  • Fixed Tu-401/TU-701 Polyurethane System
  • 20 to 30-Minute Working Window
  • Shore A 70 with 750% Elongation

Product Description

CONATHANE TU-401 / TU-701 is the Part B curative for the fixed CONATHANE TU-401 Part A plus TU-701 Part B polyurethane system. The unfilled, 100% solids formulation supports casting and potting processes for flexible molds, industrial wheels, pads, gaskets, bushings and damping components, with room-temperature and elevated-temperature cure options. Documented applications include flexible molds and tooling, industrial wheels, pads and bushings, and gaskets and damping pads. The TU-401 / TU-701 system can be processed by hand mixing, meter mixing or vacuum potting and casting.

Key features

  • Mix ratio: Fixed TU-401 Part A / TU-701 Part B polyurethane system with a 100:65 mix ratio by weight.
  • Processing window: 20-30 minute work life at 25 C with room-temperature or 80 C cure options.
  • Mechanical performance: Cured system provides Shore A 70 hardness, 750% elongation and 8,000-hour ASTM G53 UV exposure without visual degradation.

Applications

  • Flexible molds and tooling
  • Industrial wheels, pads and bushings
  • Gaskets and damping pads
Product Family

CONATHANE TU-701

Loading pricing…

TDS, SDS & Technical Documents

Technical Specifications

General Properties
Component System
Describes the number of components that must be supplied, mixed, or activated before application or cure.
2 Part
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.04
Work life @25°C
Work life is the amount of time we have to work with a material until it is no longer able to be easily worked and applied on a substrate. It is based on the change in viscosity and it can rely on the application requirements.
0.33-0.5 hours
Electrical Properties
Arc Resistance
ASTM-D495 expresses arc resistance as the number of seconds that a material resists forming a surface-conducting path when exposed to a high-voltage, low-current arc occurring intermittently. Results obtained from a nominal 3 mm thickness are meant to represent the material’s reaction in any thickness.
>120 s
Volume Resistivity
Volume resistivity, also called volume resistance, bulk resistance or bulk resistivity is a thickness dependent measurement of the resistivity of a material perpendicular to the plane of the surface.
3.4E11 Ohms⋅cm

Additional Information

Tooling & Moldmaking Materials

TU-701 Part B curative for the fixed TU-401 / TU-701 tooling elastomer system

CONATHANE TU-701 is the Part B curative for the fixed CONATHANE TU-401 Part A plus TU-701 Part B polyurethane system. The unfilled, 100% solids formulation supports casting and potting processes for flexible molds, industrial wheels, pads, gaskets, bushings and damping components, with room-temperature and elevated-temperature cure options.

100:65 mix by weight20-30 min work lifeShore A 70 cured750% elongation

As-Supplied Properties

Component and mixed-material properties

Keep component properties distinct from mixed-system values. The values below are typical and apply at the stated conditions.

Property TU-701 Part B Curative TU-401 Part A Prepolymer Condition / Basis
Viscosity 400 cP 8,500 cP 25 deg C
Specific gravity 1.01 1.04 25 deg C
Appearance Clear amber Clear light amber As supplied
Mix ratio 65 parts by weight; 67 parts by volume 100 parts by weight; 100 parts by volume Fixed TU-401 / TU-701 system
Initial mixed viscosity 2,000 cP - 25 deg C
Work life 20-30 minutes - 25 deg C

Typical values are not intended for specification use.

Processing

Mixing, de-airing and cure

The TU-401 / TU-701 system can be processed by hand mixing, meter mixing or vacuum potting and casting. The cure schedules are recommendations and should be optimized for the application.

  1. Mix TU-401 Part A and TU-701 Part B at 100:65 by weight or 100:67 by volume until homogeneous.
  2. Components may be preheated up to 60 deg C when reduced viscosity is required.
  3. For hand mixing, degas the mixed material at greater than 27 in. Hg vacuum before use.
  4. Cure for 7-21 days at 25 deg C or 16 hours at 80 deg C.

Demold and cure windows

  • Demold: 24 hours at 25 deg C or 2 hours at 80 deg C.
  • Cure time is based on time after the unit reaches the specified temperature.
  • Use only the fixed TU-401 Part A and TU-701 Part B pairing for the mixed and cured values shown on this page.

Storage and Handling

Protect the components from moisture during storage and use

Both components should be stored in a dry, controlled environment below 25 deg C and out of direct sunlight.

  • Original sealed containers: 12 months from date of shipment when stored as recommended.
  • The material is sensitive to moisture and atmospheric humidity.
  • Once opened, use immediately or blanket with dry air or nitrogen before resealing.
  • Mix individual components thoroughly before use.

Technical Guidance

System boundary and process control

This page is component-focused on TU-701 Part B, while mixed and cured properties are presented only for the fixed TU-401 Part A plus TU-701 Part B system.

Part B is not a standalone cured system

Use TU-701 Part B only with the fixed TU-401 Part A counterpart when applying the mix ratio, work-life, cure and final-property data shown here.

Cure schedule selection

The room-temperature and 80 deg C cure schedules are recommendations. Determine the optimum cure conditions for the specific casting geometry and process.

Final-State Properties

Typical cured TU-401 / TU-701 system properties

These mechanical and electrical values apply to the mixed and cured fixed system under the source conditions.

Property Typical Value Method / Condition
Shore hardness A 70 ASTM D2240, 25 deg C
Tensile strength 3,000 psi ASTM D412, 25 deg C
100% / 200% / 300% modulus 300 / 500 / 650 psi ASTM D412, 25 deg C
Ultimate elongation 750% ASTM D412, 25 deg C
Graves tear strength 280 pli ASTM D412, 25 deg C
Linear shrinkage <0.5% at 25 deg C cure; 1.0% at 80 deg C cure ASTM D2566
UV resistance 8,000 hours without visual degradation ASTM G53 Weatherometer
Dielectric strength 500 V/mil ASTM D149, 1/16 in. at 25 deg C
Volume resistivity 3.4 x 1011ohm-cm ASTM D257, 25 deg C
Surface resistivity 9.4 x 1012ohms/sq. ASTM D257, 25 deg C

All listed values are typical and are not specification limits.

Applications

Casting and tooling applications

The fixed TU-401 / TU-701 polyurethane system is recommended for potting and casting uses requiring elastomeric behavior and UV stability.

Flexible molds and tooling

Use for flexible mold and casting applications where an elastomeric polyurethane system is required.

Industrial wheels, pads and bushings

Typical uses include industrial wheels, metal-forming pads and bushings.

Gaskets and damping pads

Typical uses include washers, gaskets and vibration, shock or sound damping pads.

Discuss TU-401 / TU-701 processing for your casting geometry

Krayden can help review the fixed TU-401 Part A and TU-701 Part B mix ratio, viscosity, de-airing approach, cure schedule and cured-property requirements for your tooling or casting application. Krayden can also help review the documented processing conditions and evaluation criteria before testing.

Contact Us

Leading Brands Trust in Our Products and Services