CONATHANE EN-8

Harmonization Code : 3910.00.00.90 | Silicones in Primary Forms; Others

CONATHANE EN-8

Main features

  • EN-4 System Part B
  • 15-Minute System Work Life
  • Room or Heat Cure

Product Description

CONATHANE EN-8 Curative (Part B) is the Part B curative used with CONATHANE EN-4 Part A to form a non-MBOCA, two-component polyurethane potting and molding system. The amber liquid has a viscosity of 1,000 cP and a specific gravity of 1.00 at 25 deg C. When combined with EN-4 Part A at 100:17.5 by weight, the system provides a 15-minute working life and can cure at room temperature or with heat. Final properties apply to the complete EN-4/EN-8 system, not to the curative alone.

Key features

  • Part B System Curative: completes the polyurethane system when mixed with EN-4 Part A
  • 15-Minute System Work Life: provides a defined processing window after mixing with EN-4 Part A
  • Room or Heat Cure: supports ambient cure or accelerated cure schedules in the complete system

Applications

Part B curative for cable, connector, module, wire-wound-device and printed-circuit potting systems using EN-4 Part A.

Technical Specifications

General Properties
Appearance
Appearance at room temperature.
Amber Liquid
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1
Physical Properties
Viscosity (Part B)
1,000 mPa.s
Mechanical Properties
Elongation
Elongation is the process of lengthening something. It is a percentage that measures the initial, unstressed, length compared to the length of the material right before it breaks. It is commonly referred to as Ultimate Elongation or Tensile Elongation at break.
400 %
Electrical Properties
Arc Resistance
ASTM-D495 expresses arc resistance as the number of seconds that a material resists forming a surface-conducting path when exposed to a high-voltage, low-current arc occurring intermittently. Results obtained from a nominal 3 mm thickness are meant to represent the material’s reaction in any thickness.
>120 s
Dielectric Strength
Dielectric strength is measured in kV per mm and is calculated by the Breakdown voltage divided by the thickness of the tested material. Those two properties go hand in hand and while Breakdown voltage is always thickness dependent, dielectric strength is a general material property. As an example, the dielectric strength of Polyimide is 236 kV/mm. If we place 1mm of Polyimide between two electrodes, it will act as an insulator until the voltage between the electrodes reaches 236 kV. At this point it will start acting as a good conductor, causing sparks, potential punctures and current flow.
31 kV/mm
Surface Resistivity
>1.0x10^15 Ohms/sq
Volume Resistivity
Volume resistivity, also called volume resistance, bulk resistance or bulk resistivity is a thickness dependent measurement of the resistivity of a material perpendicular to the plane of the surface.
>4.3x10^15 Ohms⋅cm

Additional Information

Potting, encapsulants and underfills

CONATHANE® EN-8 Curative for the EN-4 polyurethane system

CONATHANE® EN-8 is the Part B curative used with CONATHANE® EN-4 Part A Urethane Prepolymer to form a two-component, non-MbOCA-based polyurethane system for electrical and electronic potting, molding, encapsulation, and coating applications. The EN-4 plus EN-8 system provides approximately 15 minutes of working life and can cure at room temperature or through accelerated elevated-temperature schedules. Mixed and cured properties apply to the complete EN-4 plus EN-8 system and do not describe EN-8 Part B alone.

EN-8 Part B Curative Pairs with EN-4 Part A 100:17.5 by weight Approx. 15 min working life Room or heat cure Nominal Shore A 90

Technical properties

EN-8 Part B as-supplied properties

These values describe EN-8 Part B before mixing with EN-4 Part A. Mixed-material and cured properties are shown separately below.

Property Value Unit Method / condition
Appearance Amber Not applicable As supplied
Viscosity 1,000 cP 25°C
Specific gravity 1.00 Unitless 25°C
Unopened shelf stability 15 months At 25°C, from date of manufacture

EN-4 plus EN-8 system

Component and mix information

EN-8 Part B is combined with EN-4 Part A to form the complete polyurethane system. Keep the component and mixed-system values distinct when evaluating or processing the material.

Property EN-4 Part A EN-8 Part B Condition / unit
Appearance Amber liquid Amber As supplied
Viscosity 9,000 1,000 cP at 25°C
Specific gravity 0.97 1.00 25°C
NCO content 8.9 to 9.1% Not applicable As supplied
Mix ratio 100 parts EN-4 Part A : 17.5 parts EN-8 Part B By weight

Processing window

Mixed viscosity development

The EN-4 plus EN-8 system has an approximate working life of 15 minutes. The mixed viscosity increases rapidly after mixing, progressing from 5,550 cP initially to 17,000 cP after 10 minutes and reaching gel by the 20-minute measurement point at 25°C.

Property Elapsed time Typical value Condition
Mixed viscosity Initial 5,550 cP 25°C
Mixed viscosity 10 min 17,000 cP 25°C
Material state 20 min Gel 25°C
Peak exotherm 2 lb mass 55°C Mixed at 25°C

Processing distinction: The approximately 15-minute working life and the 20-minute gel measurement describe different processing points and should not be used interchangeably.

Processing

Mix, degas, cast, and cure

Prepare and combine

Mix EN-4 Part A and EN-8 Part B thoroughly at 25°C to 40°C using metal, plastic, or glass stirrers and containers. Use 100 parts EN-4 Part A to 17.5 parts EN-8 Part B by weight.

Degas

Degas the mixed material at 1 to 5 mm Hg. Use a container with sufficient capacity for material expansion during the vacuum-degassing cycle.

Cast

Pour the degassed mixed material into molds at temperatures from 25°C to 100°C. Avoid materials or containers that can introduce moisture into the polyurethane system.

Stage Temperature Recommended time
Cure 25°C 5 to 7 days
Cure 60°C 4 hours
Cure 80°C 2 hours
Cure 100°C 1 hour
Demold 60°C 2 hours
Demold 80°C 1 hour

Cured system

Typical cured properties

The bulletin reports very similar cured properties for EN-7 and EN-8 when processed as recommended. EN-8 test specimens were cured for 7 days at 25°C.

Property Typical value Unit Method / condition
Color Amber or black Not applicable Visual
Specific gravity 1.01 Unitless ASTM D792, 25°C
Hardness 90 Shore A ASTM D2240
Tensile strength >2,000 psi ASTM D412
100% modulus 800 psi ASTM D412
300% modulus 1,200 psi ASTM D412
Ultimate elongation >400 % ASTM D412
Tear strength, Die C >200 pli ASTM D624
Linear shrinkage 1.15 % Cytec / MIL-M-24041
Volumetric shrinkage 3.7 % Cytec / MIL-M-24041
Water absorption 0.20 % ASTM D570, 24 h at 25°C
Water absorption 0.43 % ASTM D570, 30 d at 25°C
Heat-aging weight loss 0.41 % MIL-M-24041, 7 d at 135°C
Shore A hardness change after heat aging +5 Shore A points 7 d at 135°C
Fungus resistance Non-nutrient Result MIL-E-5272C / MIL-STD-810B
Thermal shock Pass 10 cycles Olyphant washer, 130°C to -70°C, MIL-L-16923E
Compression set 31 % ASTM D395, Method B

Data scope: These are typical values and are not intended to serve as specifications. The source groups EN-7 and EN-8 cured properties together and states that the two systems have very similar properties when processed as recommended.

Electrical performance

Typical cured-system electrical properties

Electrical data are reported for the cured EN-7 and EN-8 polyurethane systems across temperatures up to 130°C.

Property 25°C 105°C 130°C Method
Dielectric constant, 100 Hz 3.0 4.0 3.8 ASTM D150
Dielectric constant, 1 kHz 2.9 3.8 3.8 ASTM D150
Dielectric constant, 1 MHz 2.8 3.1 3.3 ASTM D150
Dissipation factor, 100 Hz 0.032 0.030 0.032 ASTM D150
Dissipation factor, 1 kHz 0.033 0.022 0.033 ASTM D150
Volume resistivity >4.3 x 1015 4.1 x 1012 7.4 x 1011 ASTM D257, ohm-cm
Surface resistivity >1.0 x 1015 4.2 x 1012 1.6 x 1012 ASTM D257, ohms
Insulation resistance >2.5 x 1013 2.3 x 1011 2.3 x 1010 MIL-M-24041, ohms
Dielectric strength, 1/16 in 785 V/mil Not reported Not reported MIL-M-24041
Arc resistance >120 sec Not reported Not reported ASTM D495

Hydrolytic stability

Property retention during 97°C / 95% RH exposure

The EN-7 and EN-8 bulletin reports elastomer properties after continuous exposure at 97°C and 95% relative humidity. Specimens were tested within 24 hours after removal from the chamber.

Property Original 28 days 56 days 84 days 112 days Unit
Hardness 94 94 94 88 87 Shore A
Tensile strength 2,250 1,600 1,400 900 775 psi
300% modulus 1,750 1,175 1,100 800 700 psi
Ultimate elongation 400 420 430 390 370 %
Tear strength, Die C 322 281 285 197 187 pli
Dielectric constant, 1 kHz at 25°C 2.9 Not reported Not reported Not reported 3.0 Unitless
Dissipation factor, 1 kHz at 25°C 0.033 Not reported Not reported Not reported 0.030 Unitless
Volume resistivity at 25°C >4.2 x 1015 Not reported Not reported Not reported 2.8 x 1015 ohm-cm
Dielectric strength, 1/16 in 785 Not reported Not reported Not reported 566 V/mil

Data scope: Hydrolytic-stability data are presented in the source for elastomers prepared from the EN-7 and EN-8 systems rather than as separately identified EN-8-only measurements.

Adhesion data

Typical peel strength on primed substrates

The cured EN-7 and EN-8 systems show greater than 20 piw peel strength on the listed substrate and primer combinations.

Substrate Primer Typical peel strength Unit
Aluminum AD-1146-C >20 piw
Stainless steel AD-1146-C >20 piw
Neoprene DPPR-7156 >20 piw
PVC AD-1161 >20 piw

Applications

Electrical and electronic protection applications

The EN-4 plus EN-8 system is recommended for molding, potting, encapsulation, and selected bonding and coating applications.

Cables and connectors

Molding and potting of electrical cables and connectors.

Modules and wound devices

Potting and encapsulation of modules, wire-wound devices, and strain-sensitive devices.

Printed circuitry

100%-solids coatings for printed circuitry.

Staking and filleting

The adhesion and flexibility of the cured systems also support evaluation for staking and filleting adhesive applications.

Storage and handling

Maintain dry storage conditions

The stated shelf life of EN-4 Part A, EN-7 Part B, and EN-8 Part B is 15 months from date of manufacture when stored in the original unopened containers at 70°F to 85°F.

If a container is opened and only partially used, flush the container with dry nitrogen before resealing to limit moisture exposure.

EN-4 Part A may crystallize during storage or shipment. If crystallization occurs, heat EN-4 Part A to 60°C, mix thoroughly, and cool to room temperature before processing.

Discuss the EN-4 plus EN-8 system

Krayden can help evaluate the EN-4 plus EN-8 system around the approximately 15-minute working life, rapidly increasing mixed viscosity, ambient or accelerated cure schedule, electrical requirements, environmental exposure, adhesion needs, assembly geometry, and dispensing process.

Contact Us

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers