ARALDITE 2081-10

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

ARALDITE 2081-10

Main features

  • Steel-to-CFRP Acrylic Bonding
  • 10-Minute Open Time
  • Non-Flammable Bonding Formulation

Product Description

ARALDITE® 2081-10 is a fast-curing, two-part acrylic structural adhesive developed for bonding a range of plastics, composites and metals. The low-odour, non-flammable system provides a 10-minute open time and a 10-11 minute pot life for a 20 g mix at 25°C, supporting rapid assembly operations. The mixed adhesive is off-white and combines high strength with good flexibility. It can be dispensed from mixer-equipped cartridges or applied manually or robotically. Tested plastic substrates include ABS, PMMA, PVC and PC; polyolefins and other low-surface-energy materials are excluded. Proper cleaning and surface preparation remain important for durable bonds.

Key features

  • Rapid strength development: 10-minute open time; on sandblasted aluminium at 23°C, typical lap shear exceeds 1 MPa in less than 20 minutes and 10 MPa in less than 23 minutes.
  • Broad substrate range: Supports bonding of tested plastics, composites and metals; not intended for polyolefins or other low-surface-energy materials.
  • Low-odour, non-flammable formulation: Two-part acrylic system with good flexibility and an off-white mixed appearance.

Applications / Suitable for

  • Plastic bonding involving ABS, PMMA, PVC or PC.
  • Composite bonding involving CFRP and epoxy-, polyester- or vinyl ester-based GRP.
  • Metal and mixed-material assemblies involving aluminium, steel, stainless steel, copper or brass.

Technical Specifications

General Properties
Color
The color
Off-White
Pot Life
Pot life is the amount of time it takes for the viscosity of a material to double (or quadruple for lower viscosity materials) in room temperature after a material is mixed. It is closely related to work life but it is not application dependent, less precise and more of a general indication of how fast a system is going to cure.
11 minutes
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.1
Physical Properties
Viscosity (Part A)
75000 mPa.s
Viscosity (Part B)
75000 mPa.s

Additional Information

Technical properties

As-supplied and mixed properties

Values are listed in Resin / Hardener / Mixed order where applicable. Data are typical supplier values and are not guaranteed specifications.

Property Value Unit Method / condition
Colour White / Light grey / Off-white - Visual; Resin / Hardener / Mixed
Specific gravity 1.04 / 1.38 / ca. 1.1 - Resin / Hardener / Mixed
Viscosity 70-80 / 60-90 / 70-90 Pa.s At 25°C; Resin / Hardener / Mixed
Mix ratio by weight 100:13 parts Resin:Hardener
Mix ratio by volume 100:10 parts Resin:Hardener
Pot life 10-11 minutes 20 g mixed material at 25°C
Time to peak exotherm 14-18 minutes 20 g mixed material
Storage and Handling

Store sealed components in their original containers at 2-8°C for up to 24 months. The product may be brought to room temperature before use, but cumulative room-temperature exposure should not exceed six months. Prolonged exposure above 25°C reduces shelf life. Follow the expiry date on the packaging and the applicable Safety Data Sheet for handling precautions.

Product-specific technical guidance

Exposed-surface tack
Atmospheric oxygen can slow cure at exposed surfaces such as fillets, leaving them tacky even when the adhesive in the bondline is cured. The supplier states that this behaviour does not affect bonding performance. Where a tack-free exposed surface is essential before sanding or painting, review the process or adhesive selection with technical support.
Equipment cleaning
Clean tools with hot water and soap before adhesive residue has cured. Cured residue is difficult and time-consuming to remove. Where solvents are used, follow the appropriate workplace controls and avoid skin and eye contact.
Cured adhesive

Typical cured properties

Typical laboratory values for adhesive cured seven days at room temperature. Values are configuration-specific and are not design allowables or guaranteed specifications.

Property Value Unit Method / condition
Glass transition temperature - onset 35 °C DMA; cure seven days at room temperature
Glass transition temperature - peak 65 °C DMA; cure seven days at room temperature
Tensile strength 17-20 MPa ISO 527; cure seven days at room temperature; test at 23°C
Tensile modulus 700-900 MPa ISO 527; cure seven days at room temperature; test at 23°C
Elongation at break ca. 60-80 % ISO 527; cure seven days at room temperature; test at 23°C

Performance evidence

The supplier TDS includes typical joint-strength and durability testing across prepared substrates and defined laboratory conditions. The results should be used for product screening and validated in the intended joint design.

Rapid strength build
Typical lap-shear strength on sandblasted aluminium at 23°C exceeded 1 MPa in less than 20 minutes and 10 MPa in less than 23 minutes under contact pressure.
Strength thresholds are specific to the stated substrate, preparation, temperature and test definition.
Substrate and durability test coverage
Typical lap-shear performance was evaluated on prepared metals, plastics and composites, and after immersion, temperature exposure, humid-heat and cold cycling, cataplasma ageing, and a simulated 200°C coating post-cure cycle.
Each dataset uses its own substrate, surface preparation, cure and exposure conditions; the results do not establish universal joint durability.

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers