ARALDITE 2031-1

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

ARALDITE 2031-1

Main features

  • Toughened Structural Bonding
  • 60 to 70-Minute Working Window
  • High Weathering Resistance Supported by Tropical-Weathering

Product Description

ARALDITE 2031-1 is a two-component, room-temperature-curing black epoxy paste adhesive for structural bonding of metals and composites. It is toughened to form a resilient bond and has thixotropic, non-slumping behavior, including non-sag application up to 10 mm. The mixed adhesive has a 60-70 minute pot life at 25°C, while integrated spacers establish a minimum 0.05 mm bondline. It is particularly suitable for GRP, CFRP and SMC bonding, and the supplier identifies high weathering resistance for bonded-joint applications.

Key features

  • Toughened structural epoxy: Forms a resilient bond for supported metal and composite joints and is identified for high weathering resistance.
  • Thixotropic non-sag paste: Remains non-slumping and can be applied at thicknesses up to 10 mm.
  • Controlled application window: Provides a 60-70 minute pot life at 25°C and integrated spacers for a minimum 0.05 mm bondline.

Applications / Suitable for

  • Metal bonding
  • GRP bonding
  • CFRP bonding
  • SMC bonding

Technical Specifications

General Properties
Color
The color
Black
Pot Life
Pot life is the amount of time it takes for the viscosity of a material to double (or quadruple for lower viscosity materials) in room temperature after a material is mixed. It is closely related to work life but it is not application dependent, less precise and more of a general indication of how fast a system is going to cure.
65 minutes
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.3

Additional Information

As supplied

Uncured and mixed-adhesive properties

Values describe the uncured components or mixed adhesive. Approximate values are identified; pot life is based on a 100 g mix at 25°C.

Property Value Unit Method condition
Appearance Black paste — Component A, Component B and mixed adhesive; visual method A112
Specific gravity A: approx. 1.2; B: approx. 1.4; mixed: approx. 1.3 — As supplied
Rheology Thixotropic — Component A, Component B and mixed adhesive at 25°C
Pot life 60-70 min Mixed adhesive; 100 g at 25°C
Mix ratio by weight 100:120 A:B Resin:hardener
Mix ratio by volume 100:100 A:B Resin:hardener; 1:1 volume
Non-sag thickness Up to 10 mm Mixed paste adhesive
Minimum bondline thickness 0.05 mm Integrated spacers

Recommended bonding sequence: prepare, mix or dispense, apply, assemble, clamp and cure.

Recommended bonding sequence

Stage 1
Prepare the substrates
Remove oil, grease and dirt with an appropriate degreasing agent. Abrade or chemically etch where stronger and more durable joints are required, then perform a second degreasing step.
Stage 2
Mix or dispense
Mix Component A and Component B at 100:120 by weight or 100:100 by volume. Cartridge formats with mixers may be applied as ready-to-use mixed adhesive using the recommended dispensing tool.
Stage 3
Apply, assemble and cure
Apply the adhesive to the pretreated, dry surfaces, assemble and clamp promptly, and maintain even contact pressure through cure. Clean tools with hot water and soap before residue cures.
Storage and Handling

Store both components in sealed containers at room temperature and use by the expiry date shown on the label. Clean uncured residue from tools with hot water and soap before cure. Use suitable gloves, eye protection and ventilation, avoid skin contact and consult the current Safety Data Sheet for full handling requirements.

Final bonded state

Cured mechanical properties

Unless otherwise stated, values are typical laboratory results. Joint properties depend on substrate, surface preparation, bondline, cure and test configuration.

Property Value Unit Method condition
Lap shear strength >20 MPa At 25°C; method A501; specified product data
Roller peel 5 N/mm ISO 4578; sand-blasted aluminum; cure 16 h at 40°C; typical
Glass transition temperature 75 °C DMA, ISO 6721; cure 16 h at 40°C; typical
Tensile strength 23 MPa ISO 527; cure 16 h at 40°C; tested at 23°C; typical
Tensile E-modulus 1 GPa ISO 527; cure 16 h at 40°C; tested at 23°C; typical
Tensile elongation at break 12 % ISO 527; cure 16 h at 40°C; tested at 23°C; typical
Flexural strength 37 MPa ISO 178; cure 16 h at 40°C; tested at 23°C; typical
Flexural E-modulus 1.2 GPa ISO 178; cure 16 h at 40°C; tested at 23°C; typical

Weathering, ageing and fluid-exposure evidence

Condition-specific laboratory programs evaluate lap shear performance after tropical weathering, heat ageing, Cataplasma ageing and immersion in multiple media. These results apply to the stated substrates, preparation, cure and test conditions.

Tropical weathering
Lap shear was evaluated after 30, 60 and 90 days at 40°C and 92% relative humidity. ARALDITE 2031-1 is identified as having high weathering resistance.
Sand-blasted aluminum; cure 16 h at 40°C; tested at 23°C.
Heat and Cataplasma ageing
Lap shear was evaluated after 30, 60 and 90 days at 70°C and after ISO 9142/E2 Cataplasma cycles combining 70°C exposure with -20°C conditioning.
Heat-ageing cure: 16 h at 40°C. Cataplasma cure: 7 days at room temperature. Test temperature: 23°C.
Fluid immersion
Lap shear was measured after 30, 60 and 90 days at 23°C in IMS, fuel, ethyl acetate, xylene, lubricating oil, paraffin and water.
Sand-blasted aluminum; cure 16 h at 40°C; tested at 23°C.

Leading Brands Trust in Our Products and Services