ARALDITE 2015-1

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

ARALDITE 2015-1

Main features

  • 15 MPa Lap Shear
  • 45 to 55-Minute Working Window
  • Evaluation Across Metals

Product Description

ARALDITE® 2015-1 is a two-component, room-temperature-curing epoxy paste structural adhesive for GRP, SMC and dissimilar-substrate bonding. The toughened, resilient system mixes 1:1 by weight or volume and forms a beige, thixotropic adhesive that fills gaps without sagging up to 10 mm. A 100 g mix provides a 45–55 minute pot life at 25°C, while specified lap shear strength of the mixed adhesive is greater than 15 MPa at 25°C. The technical data also documents cure-rate behavior across 10–100°C and evaluates bonded-joint performance after tropical humidity exposure, fluid immersion, heat aging and thermal cycling. Proper surface degreasing and abrasion or chemical etching are recommended for the strongest and most durable joints.

Key features

  • Composite and dissimilar-material bonding: Particularly suitable for SMC and GRP, with documented test data for CFRP, metals and engineering plastics.
  • Non-sag gap filling: Thixotropic paste fills gaps up to 10 mm and supports manual or robotic application.
  • Balanced working time and strength: A 45–55 minute pot life is paired with specified lap shear strength above 15 MPa at 25°C.

Applications / Suitable for

  • SMC structural bonding
  • GRP and composite panel bonding
  • Dissimilar-substrate assemblies requiring a gap-filling paste adhesive

Technical Specifications

General Properties
Pot Life
Pot life is the amount of time it takes for the viscosity of a material to double (or quadruple for lower viscosity materials) in room temperature after a material is mixed. It is closely related to work life but it is not application dependent, less precise and more of a general indication of how fast a system is going to cure.
50 minutes
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.4

Additional Information

Technical properties

As-supplied / before-processing properties

Product data for the resin, hardener and mixed adhesive. Typical values are technical information and are not guaranteed specifications unless explicitly identified as specified.

Property Value Unit Method / condition
Product form Two-component, toughened thixotropic epoxy paste — Room-temperature-curing structural adhesive
Colour Resin: beige; hardener: beige; mixed adhesive: beige — Visual, A112
Specific gravity Resin: 1.4; hardener: 1.4; mixed adhesive: 1.4 — As supplied / mixed state
Viscosity Thixotropic for resin, hardener and mixed adhesive Pa·s At 25°C; qualitative rheology description
Mix ratio by weight 100:100 parts Resin:hardener
Mix ratio by volume 100:100 parts Resin:hardener
Pot life 45–55 minutes 100 g mixed mass at 25°C
Non-sag gap filling Up to 10 mm Thixotropic mixed adhesive
Technical properties

After-processing / final-state properties

Cured-adhesive and bonded-joint data under the stated cure and test conditions. Typical values are not universal design allowables.

Property Value Unit Method / condition
Lap shear strength >15 MPa Specified value at 25°C; A501; mixed adhesive
Tensile strength 31 MPa Typical; ISO 527; cure 16 h at 40°C; tested at 23°C
Tensile modulus 1600 MPa Typical; ISO 527; cure 16 h at 40°C; tested at 23°C
Elongation at break 4.2 % Typical; ISO 527; cure 16 h at 40°C; tested at 23°C
Glass transition temperature 78 °C Typical; DMA; cure 1 h at 80°C
Flexural strength 43 MPa Typical; ISO 178; cure 16 h at 40°C; tested at 23°C
Flexural modulus 1800 MPa Typical; ISO 178; cure 16 h at 40°C; tested at 23°C
DMA shear modulus G′ at 20°C 900 MPa Typical; ISO 6721; cure 1 h at 80°C

Leading Brands Trust in Our Products and Services