ARALDITE 2014

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

ARALDITE 2014

Main features

  • Water-Resistant Epoxy Bonding
  • Up to 0.197-Inch Gap Bonding
  • Low-Outgassing Vacuum Bonding

Product Description

ARALDITE® 2014 is a two-component, room-temperature-curing epoxy paste structural adhesive for bonding metals, electronic components, GRP structures and other assemblies exposed to elevated temperatures or aggressive service environments. The grey mixed adhesive is thixotropic, fills gaps without sagging up to 0.197 in (5 mm), and has an approximate 40-minute pot life for a 100 g mix at 77°F. It combines high strength with low shrinkage and documented resistance to water and multiple chemicals. Low outgassing also supports specialist electronic, telecommunications and aerospace bonding applications. The mix ratio is 2:1 resin to hardener by weight or volume.

Key features

  • Environmental resistance: High-temperature and chemical resistance with documented water and chemical-immersion performance.
  • Controlled gap filling: Thixotropic, non-sagging paste fills gaps up to 0.197 in (5 mm).
  • Low-outgassing formulation: Suitable for specialist electronic, telecommunications and aerospace bonding applications.

Applications / Suitable for

  • Metal and GRP structural bonding
  • Electronic component assembly
  • Specialist telecommunications and aerospace bonding where low outgassing is relevant

Technical Specifications

General Properties
Pot Life
Pot life is the amount of time it takes for the viscosity of a material to double (or quadruple for lower viscosity materials) in room temperature after a material is mixed. It is closely related to work life but it is not application dependent, less precise and more of a general indication of how fast a system is going to cure.
40 minutes
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.6
Physical Properties
Viscosity (Part A)
100000 mPa.s

Additional Information

As supplied

Uncured and mixed properties

Typical as-supplied and mixed values. Values are not guaranteed specifications and should be reviewed with the applicable processing conditions.

Property Value Unit Method / condition
Product form and color Part A: beige paste; Part B: grey paste; mixed: grey paste — Visual; as supplied and mixed states
Specific gravity Part A: ~1.6; Part B: ~1.6; mixed: ~1.6 — Approximate values
Viscosity / rheology Part A: ~100,000; Part B: thixotropic; mixed: thixotropic cP At 77°F; no single numeric viscosity reported for Part B or the mixed adhesive
Mix ratio 100:50 (2:1), Part A:Part B parts By weight and by volume
Pot life ~40 minutes 100 g mixed quantity at 77°F
Gap-filling capability Up to 0.197 (5) in (mm) Non-sagging paste
Shelf life 3 years Part A and Part B in sealed containers; 36–104°F
Final bonded state

Cured physical and mechanical properties

Typical laboratory values. Cure schedule, specimen preparation, substrate and test temperature materially affect the result.

Property Value Unit Method / condition
Glass transition temperature (DSC) ~185 (85) °F (°C) Cure: 24 h at 73°F plus 1 h at 176°F
E-modulus 580,151 (4) psi (GPa) ISO R527 at 73°F
Flexural strength 8,847 (61) psi (MPa) ISO 178; cure 16 h at 104°F; tested at 73°F
Flexural modulus 631,475 (4,355) psi (MPa) ISO 178; same cure and test conditions as flexural strength
Tensile strength 3,773 (26) psi (MPa) ISO R527 at 73°F
Elongation at break 0.7 % Cured adhesive
Shear modulus 50°C: 1.2 GPa; 75°C: 400 MPa; 100°C: 180 MPa; 125°C: 20 MPa — DIN 53445; cure 16 h at 104°F
Roller peel strength 17 pli ISO 4578; cure 16 h at 104°F

Average lap shear strength by substrate

Typical ISO 4587 values for the listed prepared substrates. These results are specific to the stated surface preparation, cure and test conditions.

Property Value Unit Method / condition
Aluminum 2,762 psi ISO 4587; sandblasted; cure 16 h at 104°F; tested at 73°F
Steel 37/11 2,487 psi ISO 4587; sandblasted; cure 16 h at 104°F; tested at 73°F
Stainless steel V4A 3,149 psi ISO 4587; sandblasted; cure 16 h at 104°F; tested at 73°F
Galvanized steel 1,321 psi ISO 4587; sandblasted; cure 16 h at 104°F; tested at 73°F
Copper 2,358 psi ISO 4587; sandblasted; cure 16 h at 104°F; tested at 73°F
Brass 2,347 psi ISO 4587; sandblasted; cure 16 h at 104°F; tested at 73°F
GRP 1,247 psi ISO 4587; lightly abraded and alcohol degreased; cure 16 h at 104°F; tested at 73°F
CFRP 1,944 psi ISO 4587; lightly abraded and alcohol degreased; cure 16 h at 104°F; tested at 73°F
SMC 1,204 psi ISO 4587; lightly abraded and alcohol degreased; cure 16 h at 104°F; tested at 73°F
ABS 450 psi ISO 4587; lightly abraded and alcohol degreased; cure 16 h at 104°F; tested at 73°F
PVC 421 psi ISO 4587; lightly abraded and alcohol degreased; cure 16 h at 104°F; tested at 73°F
PMMA 218 psi ISO 4587; lightly abraded and alcohol degreased; cure 16 h at 104°F; tested at 73°F
Polycarbonate 435 psi ISO 4587; lightly abraded and alcohol degreased; cure 16 h at 104°F; tested at 73°F
Polyamides 363 psi ISO 4587; lightly abraded and alcohol degreased; cure 16 h at 104°F; tested at 73°F

Environmental exposure test results

The following typical lap shear results show tested bonded-joint behavior after chemical, water, tropical-weathering and heat-aging exposure. They are laboratory results for the stated specimens and conditions, not universal design values.

Chemical immersion
After 90 days at 73°F, reported lap shear values included 2,799 psi in IMS, 3,191 psi in gasoline, 3,336 psi in ethyl acetate, 2,321 psi in 10% acetic acid, 2,741 psi in xylene, 2,357 psi in lubricating oil and 2,756 psi in paraffin.
Cure: 16 h at 104°F. Typical average values; as-made reference: 2,764 psi.
Water immersion
After 90 days, reported lap shear was 2,450 psi in water at 73°F, 2,812 psi in water at 140°F and 2,094 psi in water at 194°F.
Cure: 16 h at 104°F. Typical average values.
Tropical weathering
Lap shear values were 2,708 psi as made, 3,078 psi after 30 days, 3,191 psi after 60 days and 2,901 psi after 90 days.
40/92 tropical weathering, DIN 50015; cure 16 h at 104°F; tested at 73°F.
Heat aging
Lap shear values were 2,712 psi as made, 2,843 psi after 30 days, 2,654 psi after 60 days and 3,017 psi after 90 days at 158°F.
Cure: 16 h at 104°F. Typical average values.

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers