ARALDITE 2012

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

ARALDITE 2012

Main features

  • 20-Minute Working Window
  • High-Strength Structural Bonding
  • Broad Substrate Range

Product Description

ARALDITE 2012 is a rapid-curing, two-component epoxy adhesive for structural and multipurpose bonding at room temperature. The high-viscosity system mixes 1:1 by weight or volume and provides a four-minute pot life for fast assembly work. It develops high shear and peel strength with a tough, resilient cured bond and is suitable for joining metals, ceramics, glass, rubbers, rigid plastics, and other common materials. Application guidance recommends clean, dry, properly prepared surfaces, a 0.05–0.10 mm adhesive layer, prompt assembly, and even contact pressure. At 23°C, typical lap shear strength exceeds 1 N/mm² after 20 minutes and 10 N/mm² after 61 minutes under the stated test method.

Key features

  • Rapid strength development: Four-minute pot life with typical lap shear strength above 1 N/mm² after 20 minutes at 23°C.
  • Tough structural bond: Documented high shear and peel strength with a tough, resilient cured adhesive.
  • Multi-material bonding: Suitable for metals, ceramics, glass, rubbers, rigid plastics, and other commonly used materials.

Applications / Suitable for

  • Metal-to-metal assembly and repair bonding
  • Glass and ceramic component bonding
  • Rubber and rigid-plastic bonding in industrial and workshop applications

Technical Specifications

General Properties
Pot Life
Pot life is the amount of time it takes for the viscosity of a material to double (or quadruple for lower viscosity materials) in room temperature after a material is mixed. It is closely related to work life but it is not application dependent, less precise and more of a general indication of how fast a system is going to cure.
4 minutes
Specific Gravity
Specific gravity (SG) is the ratio of the density of a substance to the density of a reference substance; equivalently, it is the ratio of the mass of a substance to the mass of a reference substance for the same given volume. For liquids, the reference substance is almost always water (1), while for gases, it is air (1.18) at room temperature. Specific gravity is unitless.
1.18
Physical Properties
Viscosity (Part A)
35000 mPa.s
Viscosity (Part B)
30000 mPa.s

Additional Information

Technical properties

As-supplied / before-processing properties

Typical product data for the individual components and mixed adhesive. Values are technical information, not guaranteed specifications.

Property Value Unit Method / condition
Product form Two-component, high-viscosity liquid adhesive — Room-temperature-curing epoxy system
Colour Part A: opaque; Part B: pale yellow; mixed: pale yellow — Visual
Specific gravity Part A: 1.16–1.18; Part B: 1.15–1.18; mixed: approx. 1.18 — As supplied
Viscosity Part A: 25–45; Part B: 20–40; mixed: typically 25–35 Pa·s Product data; test method and temperature not stated
Mix ratio 100:100 parts By weight and by volume; blend until homogeneous
Pot life 4 min 100 g mixed quantity at 25°C
Shelf life 3 years Parts A and B stored sealed at 2–40°C; expiry date shown on label
Technical properties

After-processing / final-state properties

Typical laboratory results for cured adhesive or bonded-joint specimens. Test method, cure schedule, and temperature are retained where stated.

Property Value Unit Method / condition
Time to lap shear strength >1 N/mm² 20 min Cure at 23°C; minimum shear-strength test
Time to lap shear strength >10 N/mm² 61 min Cure at 23°C; minimum shear-strength test
Roller peel strength 3.5 / 5.5 / 5.5 N/mm ISO 4578; cures of 48 h at 20°C / 16 h at 40°C / 2 h at 80°C
Flexural strength 46.0 MPa ISO 178; cured 16 h at 40°C and tested at 23°C
Flexural modulus 1654.4 MPa ISO 178; cured 16 h at 40°C and tested at 23°C

Leading Brands Trust in Our Products and Services