ABLESTIK 60L

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

ABLESTIK 60L

Main features

  • 50 ohm-cm Volume Resistivity
  • 30-Minute 25 deg C Cure
  • 55 to 130 deg C Service Range

Product Description

LOCTITE ABLESTIK 60L Parts AB is a black, carbon-filled, two-component epoxy adhesive for electrically conductive general-purpose bonding. The resin and amine hardener are mixed at 100:15 by weight and provide a typical one-hour work life at 25 degC for a 100 g mass. The adhesive can be cured at room temperature or with heat and is documented for an operating-temperature range of -55 to 130 degC. Its cured properties include 1.2 W/(m-K) thermal conductivity and 50 ohm-cm volume resistivity at 25 degC.

Key Features

  • Carbon-filled electrically conductive epoxy adhesive
  • Two-component resin and amine hardener system
  • 100:15 resin-to-hardener mix ratio by weight
  • Typical one-hour work life at 25 degC for a 100 g mixed mass
  • Room-temperature or heat-cure capability
  • Operating-temperature range of -55 to 130 degC
  • Typical cured thermal conductivity of 1.2 W/(m-K)

Applications / Suitable for

  • General-purpose electrically conductive bonding
  • Bonding applications where low electrical conductivity is acceptable
  • Assemblies requiring conductive adhesive bonding across a variety of substrates
  • Applications that do not require precise resistive properties for electrostatic-discharge control

Technical Specifications

General Properties
Density (g)
1.46 g/cm3
Mix Ratio
The amount of a constituent divided by the total amount of all other constituents in a mixture
100 : 15
Work life @25°C
Work life is the amount of time we have to work with a material until it is no longer able to be easily worked and applied on a substrate. It is based on the change in viscosity and it can rely on the application requirements.
1 hours
Thermal Properties
Operating Temperature
-55 to 130 °C
Thermal Conductivity
Thermal conductivity describes the ability of a material to conduct heat. It is required by power packages in order to dissipate heat and maintain stable electrical performance. Thermal conductivity units are [W/(m K)] in the SI system and [Btu/(hr ft °F)] in the Imperial system.
1.2 W/m.K
Electrical Properties
Volume Resistivity
Volume resistivity, also called volume resistance, bulk resistance or bulk resistivity is a thickness dependent measurement of the resistivity of a material perpendicular to the plane of the surface.
50 Ohms⋅cm

Additional Information

Carbon-Filled Electrically Conductive Epoxy Adhesive

LOCTITE ABLESTIK 60L Parts AB

LOCTITE ABLESTIK 60L Parts AB is a black, carbon-filled, two-component epoxy adhesive designed for general-purpose electrically conductive bonding. It uses an amine hardener at a 100:15 resin-to-hardener ratio by weight, provides a typical one-hour work life at 25 degC for a 100 g mass, and can be cured at room temperature or with heat.

Carbon filled Electrically conductive Two component Room-temperature or heat cure -55 to 130 degC

Component and Mixed Material Data

As-Supplied Properties

Part A is the epoxy resin and Part B is an amine hardener. Both are black pastes. Component-specific density and shelf-life values are kept separate from the mixed-material density and work life.

Typical uncured properties
Material state Property Typical value Condition / method
Part A — resin Appearance Black paste As supplied
Part A — resin Density 1.46 g/cm3 ASTM D792
Part A — resin Shelf life 274 days 25 degC, from date of manufacture
Part B — hardener Appearance Black paste Amine hardener
Part B — hardener Density 1.35 g/cm3 ASTM D792
Part B — hardener Shelf life 274 days 25 degC, from date of manufacture
Mixed material Density 1.46 g/cm3 ASTM D792
Mixed material Work life 1 hour 100 g mass at 25 degC

Preparation, Mixing and Cure

Mixing and Cure

Clean substrates thoroughly to remove oxide layers, dust, moisture, salt, oils, and other contamination. Because component separation can occur during shipping and storage, remix each shipping container thoroughly before measuring. Accurately weigh resin and hardener at 100:15 by weight, then blend for 2 to 3 minutes using a kneading motion while scraping the sides and bottom of the mixing container.

Mix ratio100 parts resin to 15 parts hardener by weight.
Room-temperature cure24 hours at 25 degC.
Heat-cure option 11 hour at 65 degC.
Heat-cure option 230 minutes at 100 degC.
Post-cure guidanceFor optimum performance, follow the initial cure with 2 to 4 hours at the maximum expected operating temperature.

Cure profiles are guideline recommendations and may require adjustment for the application, equipment, oven loading, and actual material temperature.

Storage and Handling

The TDS specifies a maximum storage temperature of 25 degC for the unopened product in a dry location, with a typical shelf life of 274 days at 25 degC for both Part A and Part B. Keep containers closed and do not return removed material to the original container. The supplied U.S. Part B SDS likewise specifies storage at or below 25 degC and avoidance of moisture.

Final Cured Adhesive

Cured Properties

The cured adhesive provides a carbon-filled conductive path with moderate bulk thermal conductivity and documented mechanical strength. The values below are typical laboratory results and should not be treated as guaranteed system-level performance.

Thermal conductivity
1.2 W/(m-K)

ASTM D2214.

Volume resistivity
50 ohm-cm

ASTM D257 at 25 degC.

Operating range
-55 to 130 degC

Documented product operating-temperature range.

Typical cured material and bonded-joint performance
Property Typical result Method / condition
Thermal conductivity 1.2 W/(m-K) ASTM D2214
Flexural strength 41 N/mm2 (6,000 psi) ASTM D1184
Volume resistivity 50 ohm-cm ASTM D257, 25 degC
Tensile lap shear strength 10.4 N/mm2 (1,500 psi) ASTM D1002, aluminum-to-aluminum at 25 degC

Documented Use Scope

Applications

General Conductive Bonding

Designed for general-purpose bonding where an electrically conductive carbon-filled epoxy is appropriate.

Broad Substrate Bonding

The manufacturer states that the material adheres well to a variety of substrates. Exact material compatibility should be confirmed for the intended surface, finish, preparation, and service environment.

Non-Precision Resistive Applications

The TDS explicitly states that the product is not intended where precise resistive properties, such as electrostatic-discharge control, are required.

Technical Support for LOCTITE ABLESTIK 60L Parts AB

Discuss component handling, mix-ratio control, working time, substrate preparation, cure profiling, conductive-joint requirements, and application validation with Krayden. Trials should confirm adhesion, electrical behavior, thermal performance, and mechanical strength in the intended assembly.