3M TC-2810

Harmonization Code : 3214.10.00 | Putty and other mastics | Resin cements, caulking compounds and other mastics

3M TC-2810

Main features

  • Thermally Conductive Insulation
  • Extended Assembly Work Life
  • Pre-Assembly Tack and Gap Fill

Product Description

3M Thermally Conductive Epoxy Adhesive TC-2810 is a two-part boron-nitride-filled epoxy adhesive for thermally conductive, electrically insulating bonding. The 2:1 by-volume mix provides a typical 100 to 120 minute work life at 23 deg C and slight tack for pre-assembly. Mixed viscosity is 40,000 to 80,000 cP, supporting gap filling, potting, and thin bondline application. Typical cured thermal conductivity is 0.80 to 1.4 W/(m K), with volume resistivity of 1.5 x 10^14 ohm cm. Multiple ambient and heat-cure schedules allow the process to be matched to the assembly.

Key features

  • Thermally conductive insulation: Ceramic filler combines a typical 0.80 to 1.4 W/(m K) cured value with electrical insulation.
  • Extended assembly work life: A typical 100 to 120 minute window at 23 deg C supports placement and pre-assembly.
  • Gap filling with pre-assembly tack: Mixed flow supports potting and thin bondlines, while slight tack holds parts before cure.

Applications

Applications include LED assembly, electrically insulating thermal bonding, potting, and general gap filling.

Technical Specifications

Physical Properties
Viscosity (Part A)
Base: 40000-90000 mPa.s
Viscosity (Part B)
Accelerator: 11000-21000 mPa.s
General Properties
Component System
Describes the number of components that must be supplied, mixed, or activated before application or cure.
Base Resin: Epoxy | Accelerator: Amine
Filler Content
Ceramic: 24 %

Additional Information

Technical properties

As-supplied / before-processing properties

Viscosity values are typical and remain separated by base, accelerator, and mixed state.

PropertyValueUnitMethod / condition
Base viscosity40,000 to 90,000cP40 mm, 2 deg cone at 10 s^-1
Accelerator viscosity11,000 to 21,000cP40 mm, 2 deg cone at 10 s^-1
Mixed viscosity40,000 to 80,000cP40 mm, 2 deg cone at 10 s^-1
Ceramic filler content24wt%As supplied
Mix ratio, B:A2:1by volumeTwo-part system
Work life100 to 120minutes23 deg C
Technical properties

After-processing / final-state properties

Cured values are typical and depend on the stated method and cure schedule.

PropertyValueUnitMethod / condition
Thermal conductivity0.80 to 1.4W/(m K)ASTM D5470; cured material
Volume resistivity1.5 x 10^14ohm cmASTM D257
Dielectric breakdown voltage44.0kV/mmASTM D149
Dielectric constant4.1ASTM D150
Overlap shear strength18.62N/mm^2ASTM D1002; 23 deg C/24 h, 90 deg C/30 min, or 120 deg C/10 min cure
Shore D hardness75 / 80 / 80ASTM D2240; same three cure schedules in listed order

Leading Brands Trust in Our Products and Services