3M DP8610NS

Harmonization Code : 3907.30.00.40 | Epoxy Mold Compounds containing by weight more than 70 % silicon dioxide

3M DP8610NS

Main features

  • Flexible Dissimilar Material Bonding
  • Non Sag Bondline Control
  • Fast Handling Strength Development

Product Description

3M Scotch-Weld Flexible Acrylic Adhesive DP8610NS is a black, low-odor, non-flammable two-part acrylic structural adhesive with a 10:1 mix ratio. The non-sag formulation and internal spacer beads support controlled bondline placement on panels, frames, thin materials, and dissimilar substrates. A 7 minute work life and 20 minute handling-strength time support fast room-temperature assembly. After cure, the flexible adhesive provides 140% elongation and qualified overlap-shear performance across metals, plastics, and fiber-reinforced composites for efficient industrial panel assembly.

Key features

  • Flexible Dissimilar Material Bonding: The acrylic system bonds compatible metals, plastics, and composite panels.
  • Non Sag Bondline Control: Thixotropic flow and spacer beads support consistent adhesive placement.
  • Fast Handling Strength Development: The mixed adhesive reaches handling strength in about 20 minutes at 23 deg C.

Applications

Panel and frame bonding, thin-panel assembly, and joining compatible dissimilar substrates in transportation and industrial structures.

Technical Specifications

General Properties
Component System
Describes the number of components that must be supplied, mixed, or activated before application or cure.
Two (Base / Accelerator)
Other Properties
Storage Temperature
16 - 27 °C
Thermal Properties
Glass Transition Temperature (Tg)
The glass transition temperature for organic adhesives is a temperature region where the polymers change from glassy and brittle to soft and rubbery. Increasing the temperature further continues the softening process as the viscosity drops too. Temperatures between the glass transition temperature and below the decomposition point of the adhesive are the best region for bonding. The glass-transition temperature Tg of a material characterizes the range of temperatures over which this glass transition occurs.
27 °C
Thermal Conductivity
Thermal conductivity describes the ability of a material to conduct heat. It is required by power packages in order to dissipate heat and maintain stable electrical performance. Thermal conductivity units are [W/(m K)] in the SI system and [Btu/(hr ft °F)] in the Imperial system.
0.235 W/m.K

Additional Information

Technical properties

As-supplied / before-processing properties

PropertyValueUnitMethod / condition
Mix ratio by volume10:1B:ATwo-part system
Mix ratio by weight10:1B:ATwo-part system
Base colorBlack-Before mixing
Accelerator colorGray-Before mixing
Base viscosity35000 to 100000cPAt 23 deg C; cone-and-plate, 4 sec^-1
Accelerator viscosity8000 to 18000cPAt 23 deg C; cone-and-plate, 4 sec^-1
Work life7minMixed adhesive
Open time8minBefore closing and fixing the bond
Technical properties

After-processing / final-state properties

PropertyValueUnitMethod / condition
ColorBlack-Cured
Modulus25MPaASTM D638 / ISO 527 at 23 deg C
Elongation at break140%ASTM D638 / ISO 527 after 7 days
Hardness38Shore DASTM D2240 at 23 deg C
Overlap shear on aluminum6.8MPaASTM D1002; MEK, abrade, MEK; 72 h at 23 deg C
Overlap shear on fiber-reinforced epoxy10.1MPaASTM D1002; MEK, abrade, MEK; 72 h at 23 deg C